Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 19.1 % Show Material materials with Dehnung of 19.1 % | Predicted Value, Transverse | |||
19.5 % Show Material materials with Dehnung of 19.5 % | Predicted Value, A80 | ||||
19.9 % Show Material materials with Dehnung of 19.9 % | Predicted Value, A80 Transverse | ||||
23 % Show Material materials with Dehnung of 23 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate | A200 | |
24.9 % Show Material materials with Dehnung of 24.9 % | Predicted Value | ||||
27 % Show Material materials with Dehnung of 27 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate | A50 | |
Elastizitätsmodul | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel | |||
Flächenreduzierung | 42.7 % Show Material materials with Flächenreduzierung of 42.7 % | Predicted Value | |||
43.0 % Show Material materials with Flächenreduzierung of 43.0 % | Predicted Value, Transverse | ||||
Härte, Brinell | 241 [-] Show Material materials with Härte, Brinell of 241 [-] | Predicted Value, Transverse | |||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | |||
Scherfestigkeit | 504.6 MPa Show Material materials with Scherfestigkeit of 504.6 MPa | Predicted Value | |||
Schubmodule | 79.4 GPa Show Material materials with Schubmodule of 79.4 GPa | Predicted Value | |||
Streckgrenze | 205 MPa Show Material materials with Streckgrenze of 205 MPa | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate | RP02 |
261.6 MPa Show Material materials with Streckgrenze of 261.6 MPa | Predicted Value, RP05 | ||||
271.2 MPa Show Material materials with Streckgrenze of 271.2 MPa | Predicted Value, RP1 | ||||
318.8 MPa Show Material materials with Streckgrenze of 318.8 MPa | Predicted Value, RP1 Transverse | ||||
358.9 MPa Show Material materials with Streckgrenze of 358.9 MPa | Predicted Value, Transverse | ||||
393.8 MPa Show Material materials with Streckgrenze of 393.8 MPa | Predicted Value, RP02 Transverse | ||||
405.5 MPa Show Material materials with Streckgrenze of 405.5 MPa | Predicted Value, RP002 | ||||
Zugfestigkeit | 380 - 515 MPa Show Material materials with Zugfestigkeit of 380 - 515 MPa | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 11.83 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 11.83 1/K | Predicted Value |
Max. Betriebstemperatur | 309.6 °C Show Material materials with Max. Betriebstemperatur of 309.6 °C | Predicted Value, Long |
Spezifische Wärmekapazität | 457.4 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 457.4 J/(kg·K) | Predicted Value |
Wärmeleitfähigkeit | 40.08 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.08 W/(m·K) | Predicted Value |
Elektrisch
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kohlenstoff | 0.18 % Show Material materials with Kohlenstoff of 0.18 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate |
Mangan | 0.6 - 0.9 % Show Material materials with Mangan of 0.6 - 0.9 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate |
Silizium | 0.15 - 0.4 % Show Material materials with Silizium of 0.15 - 0.4 % | As-Rolled or Normalized and/or Stress Relieved | ASTM A516 | Plate |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |