Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Nickel Chromium Molybdenum Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Nickel Chromium Molybdenum Steel |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Nickel Chromium Molybdenum Steel |
Zugfestigkeit | 23.0 °C | 580 MPa Show Material materials with Zugfestigkeit of 580 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1E-5 - 1.3E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 1.3E-5 1/K | Typical for Nickel Chromium Molybdenum Steel |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Nickel Chromium Molybdenum Steel | |
Spezifische Wärmekapazität | 23.0 °C | 448 - 670 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 448 - 670 J/(kg·K) | Typical for Nickel Chromium Molybdenum Steel |
Wärmeleitfähigkeit | 23.0 °C | 34 - 54 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34 - 54 W/(m·K) | Typical for Nickel Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 0.4 - 0.6 % Show Material materials with Chrom of 0.4 - 0.6 % |
Kohlenstoff | 0.23 - 0.28 % Show Material materials with Kohlenstoff of 0.23 - 0.28 % |
Kupfer | 0.35 % Show Material materials with Kupfer of 0.35 % |
Mangan | 0.7 - 0.9 % Show Material materials with Mangan of 0.7 - 0.9 % |
Molybdän | 0.15 - 0.25 % Show Material materials with Molybdän of 0.15 - 0.25 % |
Nickel | 0.4 - 0.7 % Show Material materials with Nickel of 0.4 - 0.7 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.04 % Show Material materials with Schwefel of 0.04 % |
Silizium | 0.15 - 0.35 % Show Material materials with Silizium of 0.15 - 0.35 % |