Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 12.6 % Show Material materials with Dehnung of 12.6 % | Predicted Value, A200 | |||
14 % Show Material materials with Dehnung of 14 % | Quenched and Tempered | ASTM A517 | Plate | A50 | |
14.4 % Show Material materials with Dehnung of 14.4 % | Predicted Value, A80 | ||||
16 % Show Material materials with Dehnung of 16 % | Quenched and Tempered | ASTM A517 | Plate | A50 | |
18.1 % Show Material materials with Dehnung of 18.1 % | Predicted Value, Transverse | ||||
19.1 % Show Material materials with Dehnung of 19.1 % | Predicted Value | ||||
19.4 % Show Material materials with Dehnung of 19.4 % | Predicted Value, A80 Transverse | ||||
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel | |||
Flächenreduzierung | 42.5 % Show Material materials with Flächenreduzierung of 42.5 % | Predicted Value, Transverse | |||
45 % Show Material materials with Flächenreduzierung of 45 % | Quenched and Tempered | ASTM A517 | Plate | ||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | |||
Scherfestigkeit | 646.7 MPa Show Material materials with Scherfestigkeit of 646.7 MPa | Predicted Value | |||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | |||
Streckgrenze | 315.5 MPa Show Material materials with Streckgrenze of 315.5 MPa | Predicted Value, RP1 | |||
328.3 MPa Show Material materials with Streckgrenze of 328.3 MPa | Predicted Value, RP1 Transverse | ||||
405 MPa Show Material materials with Streckgrenze of 405 MPa | Predicted Value, RP05 | ||||
467.9 MPa Show Material materials with Streckgrenze of 467.9 MPa | Predicted Value, RP02 Transverse | ||||
497.1 MPa Show Material materials with Streckgrenze of 497.1 MPa | Predicted Value, Transverse | ||||
606.1 MPa Show Material materials with Streckgrenze of 606.1 MPa | Predicted Value, RP02 | ||||
620 MPa Show Material materials with Streckgrenze of 620 MPa | Quenched and Tempered | ASTM A517 | Plate | ||
690 MPa Show Material materials with Streckgrenze of 690 MPa | Quenched and Tempered | ASTM A517 | Plate | ||
740.1 MPa Show Material materials with Streckgrenze of 740.1 MPa | Predicted Value, RP002 | ||||
Zugfestigkeit | 725 - 930 MPa Show Material materials with Zugfestigkeit of 725 - 930 MPa | Quenched and Tempered | ASTM A517 | Plate | |
795 - 930 MPa Show Material materials with Zugfestigkeit of 795 - 930 MPa | Quenched and Tempered | ASTM A517 | Plate |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 - 1.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 361.5 °C Show Material materials with Max. Betriebstemperatur of 361.5 °C | Predicted Value, Long |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel |
Spezifische Wärmekapazität | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 3 S/m Show Material materials with Elektrische Leitfähigkeit of 3 S/m | Predicted Value |
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bor | 0.0005 - 0.006 % Show Material materials with Bor of 0.0005 - 0.006 % | Quenched and Tempered | ASTM A517 | Plate |
Chrom | 0.4 - 0.65 % Show Material materials with Chrom of 0.4 - 0.65 % | Quenched and Tempered | ASTM A517 | Plate |
Kohlenstoff | 0.1 - 0.2 % Show Material materials with Kohlenstoff of 0.1 - 0.2 % | Quenched and Tempered | ASTM A517 | Plate |
Kupfer | 0.15 - 0.5 % Show Material materials with Kupfer of 0.15 - 0.5 % | Quenched and Tempered | ASTM A517 | Plate |
Mangan | 0.6 - 1 % Show Material materials with Mangan of 0.6 - 1 % | Quenched and Tempered | ASTM A517 | Plate |
Molybdän | 0.4 - 0.6 % Show Material materials with Molybdän of 0.4 - 0.6 % | Quenched and Tempered | ASTM A517 | Plate |
Nickel | 0.7 - 1 % Show Material materials with Nickel of 0.7 - 1 % | Quenched and Tempered | ASTM A517 | Plate |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | Quenched and Tempered | ASTM A517 | Plate |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % | Quenched and Tempered | ASTM A517 | Plate |
Silizium | 0.15 - 0.35 % Show Material materials with Silizium of 0.15 - 0.35 % | Quenched and Tempered | ASTM A517 | Plate |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | Quenched and Tempered | ASTM A517 | Plate |
Vanadium | 0.03 - 0.08 % Show Material materials with Vanadium of 0.03 - 0.08 % | Quenched and Tempered | ASTM A517 | Plate |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |