Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A50 | 23.0 °C | 17 % Show Material materials with Dehnung A50 of 17 % | |
Elastizitätsmodul | 23.0 °C | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel |
Flächenreduzierung | 23.0 °C | 45 % Show Material materials with Flächenreduzierung of 45 % | |
Kerbschlagenergie | 23.0 °C | 27 J Show Material materials with Kerbschlagenergie of 27 J | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel |
Streckgrenze | 23.0 °C | 585 MPa Show Material materials with Streckgrenze of 585 MPa | |
Streckgrenze Rp 0,2 | 23.0 °C | 620 MPa Show Material materials with Streckgrenze Rp 0,2 of 620 MPa | |
Yield strength Rp0.02 | 23.0 °C | 585 MPa Show Material materials with Yield strength Rp0.02 of 585 MPa | |
Zugfestigkeit | 23.0 °C | 725 MPa Show Material materials with Zugfestigkeit of 725 MPa |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.015 % Show Material materials with Aluminium of 0.015 % |
Chrom | 0.75 % Show Material materials with Chrom of 0.75 % |
Kohlenstoff | 0.22 - 0.3 % Show Material materials with Kohlenstoff of 0.22 - 0.3 % |
Mangan | 0.2 - 0.6 % Show Material materials with Mangan of 0.2 - 0.6 % |
Molybdän | 0.4 - 0.6 % Show Material materials with Molybdän of 0.4 - 0.6 % |
Nickel | 3.2 - 3.7 % Show Material materials with Nickel of 3.2 - 3.7 % |
Phosphor | 0.01 % Show Material materials with Phosphor of 0.01 % |
Schwefel | 0.012 % Show Material materials with Schwefel of 0.012 % |
Vanadium | 0.04 - 0.12 % Show Material materials with Vanadium of 0.04 - 0.12 % |