Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Chromium Molybdenum Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A50 | 23.0 °C | 18 % Show Material materials with Dehnung A50 of 18 % | |
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Chromium Molybdenum Steel |
Flächenreduzierung | 23.0 °C | 45 % Show Material materials with Flächenreduzierung of 45 % | |
Kerbschlagenergie | 23.0 °C | 54 J Show Material materials with Kerbschlagenergie of 54 J | |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Streckgrenze Rp 0,2 | 23.0 °C | 415 MPa Show Material materials with Streckgrenze Rp 0,2 of 415 MPa | |
Zugfestigkeit | 23.0 °C | 585 - 760 MPa Show Material materials with Zugfestigkeit of 585 - 760 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.1E-5 - 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.4E-5 1/K | Typical for Chromium Molybdenum Steel |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Spezifische Wärmekapazität | 23.0 °C | 448 - 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Wärmeleitfähigkeit | 23.0 °C | 36 - 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Bor | 1E-3 - 3E-3 % Show Material materials with Bor of 1E-3 - 3E-3 % |
Chrom | 2.8 - 3.3 % Show Material materials with Chrom of 2.8 - 3.3 % |
Kohlenstoff | 0.1 - 0.15 % Show Material materials with Kohlenstoff of 0.1 - 0.15 % |
Mangan | 0.3 - 0.6 % Show Material materials with Mangan of 0.3 - 0.6 % |
Molybdän | 0.9 - 1.1 % Show Material materials with Molybdän of 0.9 - 1.1 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.02 % Show Material materials with Schwefel of 0.02 % |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % |
Titan | 0.02 - 0.04 % Show Material materials with Titan of 0.02 - 0.04 % |
Vanadium | 0.2 - 0.3 % Show Material materials with Vanadium of 0.2 - 0.3 % |