Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 9 - 13 % Show Material materials with Dehnung of 9 - 13 % |
Flächenreduzierung | 20.0 °C | 28 - 40 % Show Material materials with Flächenreduzierung of 28 - 40 % |
Kerbschlagenergie | 20.0 °C | 15 - 25 J Show Material materials with Kerbschlagenergie of 15 - 25 J |
Yield Strength Rp0.2, short transverse | 20.0 °C | 965 - 1380 MPa Show Material materials with Yield Strength Rp0.2, short transverse of 965 - 1380 MPa |
Zugfestigkeit | 20.0 °C | 1035 - 1450 MPa Show Material materials with Zugfestigkeit of 1035 - 1450 MPa |
Chemical properties
Property | Value |
---|---|
Chrom | 0.8 - 1.1 % Show Material materials with Chrom of 0.8 - 1.1 % |
Kohlenstoff | 0.27 - 0.33 % Show Material materials with Kohlenstoff of 0.27 - 0.33 % |
Mangan | 0.4 - 0.6 % Show Material materials with Mangan of 0.4 - 0.6 % |
Molybdän | 0.15 - 0.25 % Show Material materials with Molybdän of 0.15 - 0.25 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 0.2 - 0.35 % Show Material materials with Silizium of 0.2 - 0.35 % |
Vanadium | 0.05 - 0.1 % Show Material materials with Vanadium of 0.05 - 0.1 % |