Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 6 - 13 % Show Material materials with Dehnung of 6 - 13 % |
Flächenreduzierung | 20.0 °C | 25 - 40 % Show Material materials with Flächenreduzierung of 25 - 40 % |
Kerbschlagenergie | 20.0 °C | 15 - 45 J Show Material materials with Kerbschlagenergie of 15 - 45 J |
Yield Strength Rp0.2, short transverse | 20.0 °C | 965 - 1550 MPa Show Material materials with Yield Strength Rp0.2, short transverse of 965 - 1550 MPa |
Zugfestigkeit | 20.0 °C | 1035 - 1720 MPa Show Material materials with Zugfestigkeit of 1035 - 1720 MPa |
Chemical properties
Property | Value |
---|---|
Chrom | 0.9 - 1.2 % Show Material materials with Chrom of 0.9 - 1.2 % |
Kohlenstoff | 0.45 - 0.5 % Show Material materials with Kohlenstoff of 0.45 - 0.5 % |
Mangan | 0.6 - 0.9 % Show Material materials with Mangan of 0.6 - 0.9 % |
Molybdän | 0.9 - 1.1 % Show Material materials with Molybdän of 0.9 - 1.1 % |
Nickel | 0.4 - 0.7 % Show Material materials with Nickel of 0.4 - 0.7 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 0.15 - 0.3 % Show Material materials with Silizium of 0.15 - 0.3 % |
Vanadium | 0.08 - 0.15 % Show Material materials with Vanadium of 0.08 - 0.15 % |