Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 8 - 9 % Show Material materials with Dehnung of 8 - 9 % |
Flächenreduzierung | 20.0 °C | 25 - 30 % Show Material materials with Flächenreduzierung of 25 - 30 % |
Kerbschlagenergie | 20.0 °C | 20 J Show Material materials with Kerbschlagenergie of 20 J |
Yield Strength Rp0.2, short transverse | 20.0 °C | 1380 - 1550 MPa Show Material materials with Yield Strength Rp0.2, short transverse of 1380 - 1550 MPa |
Zugfestigkeit | 20.0 °C | 1790 - 1930 MPa Show Material materials with Zugfestigkeit of 1790 - 1930 MPa |
Chemical properties
Property | Value |
---|---|
Chrom | 4.75 - 5.25 % Show Material materials with Chrom of 4.75 - 5.25 % |
Kohlenstoff | 0.38 - 0.43 % Show Material materials with Kohlenstoff of 0.38 - 0.43 % |
Mangan | 0.2 - 0.4 % Show Material materials with Mangan of 0.2 - 0.4 % |
Molybdän | 1.2 - 1.4 % Show Material materials with Molybdän of 1.2 - 1.4 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 0.8 - 1 % Show Material materials with Silizium of 0.8 - 1 % |
Vanadium | 0.4 - 0.6 % Show Material materials with Vanadium of 0.4 - 0.6 % |