Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A50 | 23.0 °C | 17 - 18 % Show Material materials with Dehnung A50 of 17 - 18 % | |
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel |
Flächenreduzierung | 23.0 °C | 40 - 45 % Show Material materials with Flächenreduzierung of 40 - 45 % | |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel |
Schubmodule | 23.0 °C | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel |
Streckgrenze Rp 0,2 | 23.0 °C | 620 - 690 MPa Show Material materials with Streckgrenze Rp 0,2 of 620 - 690 MPa | |
Zugfestigkeit | 23.0 °C | 725 - 930 MPa Show Material materials with Zugfestigkeit of 725 - 930 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.32E-5 - 1.38E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 - 1.38E-5 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Spezifische Wärmekapazität | 23.0 °C | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 23.0 °C | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 1.43E-7 - 1.74E-7 Ω·m Show Material materials with spezifischer Widerstand of 1.43E-7 - 1.74E-7 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Bor | 1.5E-3 - 5E-3 % Show Material materials with Bor of 1.5E-3 - 5E-3 % |
Chrom | 1.4 - 2 % Show Material materials with Chrom of 1.4 - 2 % |
Kohlenstoff | 0.12 - 0.2 % Show Material materials with Kohlenstoff of 0.12 - 0.2 % |
Kupfer | 0.2 - 0.4 % Show Material materials with Kupfer of 0.2 - 0.4 % |
Mangan | 0.4 - 0.7 % Show Material materials with Mangan of 0.4 - 0.7 % |
Molybdän | 0.4 - 0.6 % Show Material materials with Molybdän of 0.4 - 0.6 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 0.2 - 0.35 % Show Material materials with Silizium of 0.2 - 0.35 % |
Titan | 0.04 - 0.1 % Show Material materials with Titan of 0.04 - 0.1 % |