Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A50 | 23.0 °C | 14 % Show Material materials with Dehnung A50 of 14 % | |
Elastizitätsmodul | 23.0 °C | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel |
Flächenreduzierung | 23.0 °C | 50 % Show Material materials with Flächenreduzierung of 50 % | |
Härte, Brinell | 23.0 °C | 283 [-] Show Material materials with Härte, Brinell of 283 [-] | |
Härte, Rockwell C | 23.0 °C | 30 [-] Show Material materials with Härte, Rockwell C of 30 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel |
Streckgrenze | 23.0 °C | 620 MPa Show Material materials with Streckgrenze of 620 MPa | |
Zugfestigkeit | 23.0 °C | 930 MPa Show Material materials with Zugfestigkeit of 930 MPa |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.9 - 1.35 % Show Material materials with Aluminium of 0.9 - 1.35 % |
Chrom | 12.25 - 13.25 % Show Material materials with Chrom of 12.25 - 13.25 % |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Mangan | 0.2 % Show Material materials with Mangan of 0.2 % |
Molybdän | 2 - 2.5 % Show Material materials with Molybdän of 2 - 2.5 % |
Nickel | 7.5 - 8.5 % Show Material materials with Nickel of 7.5 - 8.5 % |
Phosphor | 0.01 % Show Material materials with Phosphor of 0.01 % |
Schwefel | 8E-3 % Show Material materials with Schwefel of 8E-3 % |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % |