Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.4 % Show Material materials with Dehnung of 18.4 % | Predicted Value, A200 | ||||
21.4 % Show Material materials with Dehnung of 21.4 % | Predicted Value, A5 | |||||
26.6 % Show Material materials with Dehnung of 26.6 % | Predicted Value, A50 | |||||
20 °C | 15 % Show Material materials with Dehnung of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 20 % Show Material materials with Dehnung of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 23 % Show Material materials with Dehnung of 23 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 24 % Show Material materials with Dehnung of 24 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 24 % Show Material materials with Dehnung of 24 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 26 % Show Material materials with Dehnung of 26 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel | ||||
Flächenreduzierung | 44.1 % Show Material materials with Flächenreduzierung of 44.1 % | Predicted Value, Transverse | ||||
50.8 % Show Material materials with Flächenreduzierung of 50.8 % | Predicted Value | |||||
Härte, Brinell | 249 [-] Show Material materials with Härte, Brinell of 249 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 20 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
Scherfestigkeit | 511.9 MPa Show Material materials with Scherfestigkeit of 511.9 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 263.7 MPa Show Material materials with Streckgrenze of 263.7 MPa | Predicted Value, RP1 | ||||
269.2 MPa Show Material materials with Streckgrenze of 269.2 MPa | Predicted Value, RP05 | |||||
278.1 MPa Show Material materials with Streckgrenze of 278.1 MPa | Predicted Value, Transverse | |||||
320.4 MPa Show Material materials with Streckgrenze of 320.4 MPa | Predicted Value, RP1 Transverse | |||||
349.1 MPa Show Material materials with Streckgrenze of 349.1 MPa | Predicted Value, RP02 | |||||
445.3 MPa Show Material materials with Streckgrenze of 445.3 MPa | Predicted Value, RP02 Transverse | |||||
468.1 MPa Show Material materials with Streckgrenze of 468.1 MPa | Predicted Value, RP002 | |||||
20 °C | 165 MPa Show Material materials with Streckgrenze of 165 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 175 MPa Show Material materials with Streckgrenze of 175 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 185 MPa Show Material materials with Streckgrenze of 185 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 195 MPa Show Material materials with Streckgrenze of 195 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 159 - 187 MPa Show Material materials with Streckgrenze of 159 - 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 159 - 180 MPa Show Material materials with Streckgrenze of 159 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 159 - 173 MPa Show Material materials with Streckgrenze of 159 - 173 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 159 MPa Show Material materials with Streckgrenze of 159 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 173 - 187 MPa Show Material materials with Streckgrenze of 173 - 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 173 - 180 MPa Show Material materials with Streckgrenze of 173 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 173 MPa Show Material materials with Streckgrenze of 173 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 - 187 MPa Show Material materials with Streckgrenze of 180 - 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 187 MPa Show Material materials with Streckgrenze of 187 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 - 161 MPa Show Material materials with Streckgrenze of 137 - 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 - 155 MPa Show Material materials with Streckgrenze of 137 - 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 - 149 MPa Show Material materials with Streckgrenze of 137 - 149 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 137 MPa Show Material materials with Streckgrenze of 137 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 149 - 161 MPa Show Material materials with Streckgrenze of 149 - 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 149 - 155 MPa Show Material materials with Streckgrenze of 149 - 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 149 MPa Show Material materials with Streckgrenze of 149 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 161 MPa Show Material materials with Streckgrenze of 155 - 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 MPa Show Material materials with Streckgrenze of 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 161 MPa Show Material materials with Streckgrenze of 161 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 - 143 MPa Show Material materials with Streckgrenze of 115 - 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 - 136 MPa Show Material materials with Streckgrenze of 115 - 136 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 - 129 MPa Show Material materials with Streckgrenze of 115 - 129 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 115 MPa Show Material materials with Streckgrenze of 115 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 129 - 143 MPa Show Material materials with Streckgrenze of 129 - 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 129 - 136 MPa Show Material materials with Streckgrenze of 129 - 136 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 129 MPa Show Material materials with Streckgrenze of 129 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 136 - 143 MPa Show Material materials with Streckgrenze of 136 - 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 136 MPa Show Material materials with Streckgrenze of 136 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 143 MPa Show Material materials with Streckgrenze of 143 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 - 122 MPa Show Material materials with Streckgrenze of 102 - 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 - 117 MPa Show Material materials with Streckgrenze of 102 - 117 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 - 112 MPa Show Material materials with Streckgrenze of 102 - 112 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 102 MPa Show Material materials with Streckgrenze of 102 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 112 - 122 MPa Show Material materials with Streckgrenze of 112 - 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 112 - 117 MPa Show Material materials with Streckgrenze of 112 - 117 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 112 MPa Show Material materials with Streckgrenze of 112 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 117 - 122 MPa Show Material materials with Streckgrenze of 117 - 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 117 MPa Show Material materials with Streckgrenze of 117 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 122 MPa Show Material materials with Streckgrenze of 122 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
Zugfestigkeit | 20 °C | 330 - 510 MPa Show Material materials with Zugfestigkeit of 330 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 330 - 500 MPa Show Material materials with Zugfestigkeit of 330 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 330 - 490 MPa Show Material materials with Zugfestigkeit of 330 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 330 - 480 MPa Show Material materials with Zugfestigkeit of 330 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 510 MPa Show Material materials with Zugfestigkeit of 340 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 500 MPa Show Material materials with Zugfestigkeit of 340 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 490 MPa Show Material materials with Zugfestigkeit of 340 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 340 - 480 MPa Show Material materials with Zugfestigkeit of 340 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 510 MPa Show Material materials with Zugfestigkeit of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 500 MPa Show Material materials with Zugfestigkeit of 350 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 490 MPa Show Material materials with Zugfestigkeit of 350 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 480 MPa Show Material materials with Zugfestigkeit of 350 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 510 MPa Show Material materials with Zugfestigkeit of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 500 MPa Show Material materials with Zugfestigkeit of 360 - 500 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 490 MPa Show Material materials with Zugfestigkeit of 360 - 490 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 480 MPa Show Material materials with Zugfestigkeit of 360 - 480 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 - 1.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 294.5 °C Show Material materials with Max. Betriebstemperatur of 294.5 °C | Predicted Value, Long |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel |
Spezifische Wärmekapazität | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value |
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kohlenstoff | 0.17 % Show Material materials with Kohlenstoff of 0.17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Kupfer | 0.55 % Show Material materials with Kupfer of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mangan | 1.4 % Show Material materials with Mangan of 1.4 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |