EN 12163 Grade Cu-DHP H100

View suppliers (23)
Want to keep this datasheet? Save it now in your required format

Description

Cu-DHP, mat. No CW024A, is a phosphoric pure copper grade. To the comparable DIN-mark SF-Cu, mat. No 2.0090 acc. to DIN 1787 applies: The material is a deoxidized copper with Cu >= 99,9% and a high residual copper-content. Tensile strength and Brinell hardness are increasable by cold forming. SF-Cu (Cu-DHP) is hydrogen resistant and shows the lowest thermal and electrical conductivity of the pure copper materials. Processing properties: hot forming: very good cold forming: very good machinability: unfavorable hard soldering: very good soft soldering: very good gas-shielded welding: very good burnishing: very good Application: SF-Cu is the most important copper-grade for pipes due to its very good soldering and welding properties. Further application in apparatus engineering and construction trade. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValue

Dichte

20.0 °C

8.9 - 8.94 g/cm³

Show Material materials with Dichte of 8.9 - 8.94 g/cm³

Mechanisch

PropertyTemperatureValueComment

Elastizitätsmodul

-253.0 °C

138 GPa

Show Material materials with Elastizitätsmodul of 138 GPa

-195.0 °C

136 GPa

Show Material materials with Elastizitätsmodul of 136 GPa

-100.0 °C

133 GPa

Show Material materials with Elastizitätsmodul of 133 GPa

20.0 °C

128 - 132 GPa

Show Material materials with Elastizitätsmodul of 128 - 132 GPa

50.0 °C

127 GPa

Show Material materials with Elastizitätsmodul of 127 GPa

100.0 °C

125 GPa

Show Material materials with Elastizitätsmodul of 125 GPa

150.0 °C

122 GPa

Show Material materials with Elastizitätsmodul of 122 GPa

200.0 °C

120 GPa

Show Material materials with Elastizitätsmodul of 120 GPa

250.0 °C

118 GPa

Show Material materials with Elastizitätsmodul of 118 GPa

Härte, Brinell

20.0 °C

100 [-]

Show Material materials with Härte, Brinell of 100 [-]

Härte, Vickers

20.0 °C

100 - 110 [-]

Show Material materials with Härte, Vickers of 100 - 110 [-]

Poissonzahl

20.0 °C

0.34 [-]

Show Material materials with Poissonzahl of 0.34 [-]

Schubmodule

23.0 °C

48 GPa

Show Material materials with Schubmodule of 48 GPa

Typical for Wrought Copper Pure / Low Alloyed Copper

Thermisch

PropertyTemperatureValueComment

Koeffizient der thermischen Ausdehnung

100.0 °C

1.68E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.68E-5 1/K

200.0 °C

1.73E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.73E-5 1/K

300.0 °C

1.77E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K

Unlock all property charts

Schmelzpunkt

965 - 1100 °C

Show Material materials with Schmelzpunkt of 965 - 1100 °C

Typical for Wrought Copper Pure / Low Alloyed Copper

Spezifische Wärmekapazität

-150.0 °C

282 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 282 J/(kg·K)

-50.0 °C

361 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 361 J/(kg·K)

20.0 °C

386 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 386 J/(kg·K)

100.0 °C

393 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 393 J/(kg·K)

200.0 °C

403 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 403 J/(kg·K)

300.0 °C

415 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 415 J/(kg·K)

Unlock all property charts

Wärmeleitfähigkeit

20.0 °C

305 - 340 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 305 - 340 W/(m·K)

50.0 °C

310 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 310 W/(m·K)

100.0 °C

318 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 318 W/(m·K)

200.0 °C

326 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 326 W/(m·K)

300.0 °C

334 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 334 W/(m·K)

Unlock all property charts

Elektrisch

PropertyTemperatureValue

Elektrische Leitfähigkeit

20.0 °C

4.30E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 4.30E+7 S/m

50.0 °C

4.10E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 4.10E+7 S/m

100.0 °C

3.70E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 3.70E+7 S/m

200.0 °C

3.40E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 3.40E+7 S/m

300.0 °C

3.00E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 3.00E+7 S/m

Unlock all property charts

spezifischer Widerstand

20.0 °C

2.2E-8 Ω·m

Show Material materials with spezifischer Widerstand of 2.2E-8 Ω·m

50.0 °C

2.4E-8 Ω·m

Show Material materials with spezifischer Widerstand of 2.4E-8 Ω·m

100.0 °C

2.7E-8 Ω·m

Show Material materials with spezifischer Widerstand of 2.7E-8 Ω·m

200.0 °C

2.9E-8 Ω·m

Show Material materials with spezifischer Widerstand of 2.9E-8 Ω·m

300.0 °C

3.3E-8 Ω·m

Show Material materials with spezifischer Widerstand of 3.3E-8 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Kupfer

99.9 %

Show Material materials with Kupfer of 99.9 %

Phosphor

0.02 - 0.04 %

Show Material materials with Phosphor of 0.02 - 0.04 %

Silber

0.02 %

Show Material materials with Silber of 0.02 %