Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.2 g/cm³ Show Material materials with Dichte of 8.2 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 20.0 °C | 105 GPa Show Material materials with Elastizitätsmodul of 105 GPa | |
Härte, Brinell | 20.0 °C | 190 [-] Show Material materials with Härte, Brinell of 190 [-] | |
Härte, Vickers | 20.0 °C | 200 [-] Show Material materials with Härte, Vickers of 200 [-] | |
Schubmodule | 23.0 °C | 40 GPa Show Material materials with Schubmodule of 40 GPa | Typical for Wrought Copper Brass |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 27 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 27 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 4.00E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 4.00E+6 S/m |
Specific Electrical conductivity | 6.9 % IACS Show Material materials with Specific Electrical conductivity of 6.9 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminium | 5 - 7 % Show Material materials with Aluminium of 5 - 7 % |
Blei | 0.2 - 1 % Show Material materials with Blei of 0.2 - 1 % |
Eisen | 2 - 3.5 % Show Material materials with Eisen of 2 - 3.5 % |
Kupfer | 63 - 65.5 % Show Material materials with Kupfer of 63 - 65.5 % |
Mangan | 3.5 - 5 % Show Material materials with Mangan of 3.5 - 5 % |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % |
Zinn | 0.2 % Show Material materials with Zinn of 0.2 % |