Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.67 - 8.7 g/cm³ Show Material materials with Dichte of 8.67 - 8.7 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 5 % Show Material materials with Dehnung of 5 % |
Elastizitätsmodul | 20.0 °C | 125 GPa Show Material materials with Elastizitätsmodul of 125 GPa |
Elongation A10 | 20.0 °C | 3 % Show Material materials with Elongation A10 of 3 % |
Elongation A100 | 20.0 °C | 2 % Show Material materials with Elongation A100 of 2 % |
Elongation A11.3 | 20.0 °C | 2 - 3 % Show Material materials with Elongation A11.3 of 2 - 3 % |
Poissonzahl | 20.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] |
Streckgrenze Rp 0,2 | 20.0 °C | 400 - 450 MPa Show Material materials with Streckgrenze Rp 0,2 of 400 - 450 MPa |
Zugfestigkeit | 20.0 °C | 540 MPa Show Material materials with Zugfestigkeit of 540 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 300.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | |
Schmelzpunkt | 875 - 1135 °C Show Material materials with Schmelzpunkt of 875 - 1135 °C | Typical for Wrought Copper Nickel Silver Grade | |
Spezifische Wärmekapazität | 20.0 °C | 380 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 380 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 4.40E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 4.40E+6 S/m |
Specific Electrical conductivity | 8 % IACS Show Material materials with Specific Electrical conductivity of 8 % IACS |
Chemical properties
Property | Value |
---|---|
Blei | 0.03 % Show Material materials with Blei of 0.03 % |
Eisen | 0.3 % Show Material materials with Eisen of 0.3 % |
Kupfer | 63 - 66 % Show Material materials with Kupfer of 63 - 66 % |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % |
Nickel | 11 - 13 % Show Material materials with Nickel of 11 - 13 % |
Zinn | 0.03 % Show Material materials with Zinn of 0.03 % |