Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.4 - 8.41 g/cm³ Show Material materials with Dichte of 8.4 - 8.41 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 45 % Show Material materials with Dehnung of 45 % |
150.0 °C | 52 % Show Material materials with Dehnung of 52 % | |
200.0 °C | 42 % Show Material materials with Dehnung of 42 % | |
250.0 °C | 31 % Show Material materials with Dehnung of 31 % | |
Elastizitätsmodul | -195.0 °C | 108 GPa Show Material materials with Elastizitätsmodul of 108 GPa |
-100.0 °C | 106 GPa Show Material materials with Elastizitätsmodul of 106 GPa | |
20.0 °C | 102 - 105 GPa Show Material materials with Elastizitätsmodul of 102 - 105 GPa | |
50.0 °C | 100 GPa Show Material materials with Elastizitätsmodul of 100 GPa | |
100.0 °C | 93 - 99 GPa Show Material materials with Elastizitätsmodul of 93 - 99 GPa | |
150.0 °C | 91 GPa Show Material materials with Elastizitätsmodul of 91 GPa | |
200.0 °C | 89 - 94 GPa Show Material materials with Elastizitätsmodul of 89 - 94 GPa | |
250.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | |
300.0 °C | 89 GPa Show Material materials with Elastizitätsmodul of 89 GPa | |
400.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | |
500.0 °C | 74 GPa Show Material materials with Elastizitätsmodul of 74 GPa | |
600.0 °C | 64 GPa Show Material materials with Elastizitätsmodul of 64 GPa | |
700.0 °C | 54 GPa Show Material materials with Elastizitätsmodul of 54 GPa | |
Poissonzahl | 20.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] |
Schubmodule | 20.0 °C | 37 GPa Show Material materials with Schubmodule of 37 GPa |
Streckgrenze Rp 0,2 | 20.0 °C | 223 MPa Show Material materials with Streckgrenze Rp 0,2 of 223 MPa |
150.0 °C | 232 MPa Show Material materials with Streckgrenze Rp 0,2 of 232 MPa | |
200.0 °C | 224 MPa Show Material materials with Streckgrenze Rp 0,2 of 224 MPa | |
250.0 °C | 206 MPa Show Material materials with Streckgrenze Rp 0,2 of 206 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 246 MPa Show Material materials with Streckgrenze Rp 1,0 of 246 MPa |
150.0 °C | 251 MPa Show Material materials with Streckgrenze Rp 1,0 of 251 MPa | |
200.0 °C | 243 MPa Show Material materials with Streckgrenze Rp 1,0 of 243 MPa | |
250.0 °C | 227 MPa Show Material materials with Streckgrenze Rp 1,0 of 227 MPa | |
Zugfestigkeit | 20.0 °C | 419 MPa Show Material materials with Zugfestigkeit of 419 MPa |
150.0 °C | 366 MPa Show Material materials with Zugfestigkeit of 366 MPa | |
200.0 °C | 331 MPa Show Material materials with Zugfestigkeit of 331 MPa | |
250.0 °C | 296 MPa Show Material materials with Zugfestigkeit of 296 MPa | |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 375 - 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 375 - 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 109 - 117 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 109 - 117 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.39E+7 - 1.50E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.39E+7 - 1.50E+7 S/m |
Specific Electrical conductivity | 24 - 26 % IACS Show Material materials with Specific Electrical conductivity of 24 - 26 % IACS | |
spezifischer Widerstand | 20.0 °C | 6.7E-8 Ω·m Show Material materials with spezifischer Widerstand of 6.7E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.05 % Show Material materials with Aluminium of 0.05 % |
Blei | 0.2 - 0.3 % Show Material materials with Blei of 0.2 - 0.3 % |
Eisen | 0.2 % Show Material materials with Eisen of 0.2 % |
Kupfer | 59.5 - 61.5 % Show Material materials with Kupfer of 59.5 - 61.5 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Zinn | 0.2 % Show Material materials with Zinn of 0.2 % |