Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.4 - 8.41 g/cm³ Show Material materials with Dichte of 8.4 - 8.41 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 35 - 55 % Show Material materials with Dehnung of 35 - 55 % |
150.0 °C | 62 % Show Material materials with Dehnung of 62 % | |
200.0 °C | 45 % Show Material materials with Dehnung of 45 % | |
250.0 °C | 28 % Show Material materials with Dehnung of 28 % | |
Elastizitätsmodul | -195.0 °C | 108 GPa Show Material materials with Elastizitätsmodul of 108 GPa |
-100.0 °C | 106 GPa Show Material materials with Elastizitätsmodul of 106 GPa | |
20.0 °C | 102 - 105 GPa Show Material materials with Elastizitätsmodul of 102 - 105 GPa | |
50.0 °C | 100 GPa Show Material materials with Elastizitätsmodul of 100 GPa | |
100.0 °C | 93 - 99 GPa Show Material materials with Elastizitätsmodul of 93 - 99 GPa | |
150.0 °C | 91 GPa Show Material materials with Elastizitätsmodul of 91 GPa | |
200.0 °C | 89 - 94 GPa Show Material materials with Elastizitätsmodul of 89 - 94 GPa | |
250.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | |
300.0 °C | 89 GPa Show Material materials with Elastizitätsmodul of 89 GPa | |
400.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | |
500.0 °C | 74 GPa Show Material materials with Elastizitätsmodul of 74 GPa | |
600.0 °C | 64 GPa Show Material materials with Elastizitätsmodul of 64 GPa | |
700.0 °C | 54 GPa Show Material materials with Elastizitätsmodul of 54 GPa | |
Härte, Brinell | 20.0 °C | 70 - 100 [-] Show Material materials with Härte, Brinell of 70 - 100 [-] |
Härte, Vickers | 20.0 °C | 75 - 105 [-] Show Material materials with Härte, Vickers of 75 - 105 [-] |
Poissonzahl | 20.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] |
Schubmodule | 20.0 °C | 37 GPa Show Material materials with Schubmodule of 37 GPa |
Streckgrenze Rp 0,2 | 20.0 °C | 125 - 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 125 - 250 MPa |
150.0 °C | 130 MPa Show Material materials with Streckgrenze Rp 0,2 of 130 MPa | |
200.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 0,2 of 135 MPa | |
250.0 °C | 127 MPa Show Material materials with Streckgrenze Rp 0,2 of 127 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 137 MPa Show Material materials with Streckgrenze Rp 1,0 of 137 MPa |
150.0 °C | 144 MPa Show Material materials with Streckgrenze Rp 1,0 of 144 MPa | |
200.0 °C | 146 MPa Show Material materials with Streckgrenze Rp 1,0 of 146 MPa | |
250.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 1,0 of 135 MPa | |
Zugfestigkeit | 20.0 °C | 340 - 374 MPa Show Material materials with Zugfestigkeit of 340 - 374 MPa |
150.0 °C | 314 MPa Show Material materials with Zugfestigkeit of 314 MPa | |
200.0 °C | 271 MPa Show Material materials with Zugfestigkeit of 271 MPa | |
250.0 °C | 221 MPa Show Material materials with Zugfestigkeit of 221 MPa | |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 375 - 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 375 - 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 109 - 117 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 109 - 117 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.39E+7 - 1.50E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.39E+7 - 1.50E+7 S/m |
Specific Electrical conductivity | 24 - 26 % IACS Show Material materials with Specific Electrical conductivity of 24 - 26 % IACS | |
spezifischer Widerstand | 20.0 °C | 6.7E-8 Ω·m Show Material materials with spezifischer Widerstand of 6.7E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.05 % Show Material materials with Aluminium of 0.05 % |
Blei | 0.2 - 0.3 % Show Material materials with Blei of 0.2 - 0.3 % |
Eisen | 0.2 % Show Material materials with Eisen of 0.2 % |
Kupfer | 59.5 - 61.5 % Show Material materials with Kupfer of 59.5 - 61.5 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Zinn | 0.2 % Show Material materials with Zinn of 0.2 % |