Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.83 - 8.9 g/cm³ Show Material materials with Dichte of 8.83 - 8.9 g/cm³ |
Abmessung
Property | Value | Comment | |
---|---|---|---|
Außendurchmesser | 0.76 - 76 mm Show Material materials with Außendurchmesser of 0.76 - 76 mm | Rod | |
Breite | 305 - 559 mm Show Material materials with Breite of 305 - 559 mm | ||
Dicke | 0.76 - 76 mm Show Material materials with Dicke of 0.76 - 76 mm | Bar | |
Durchmesser | 1.27 - 12.7 mm Show Material materials with Durchmesser of 1.27 - 12.7 mm | ||
Länge | 610 - 91000 mm Show Material materials with Länge of 610 - 91000 mm | max. Rod and Bar | |
Wall thickness | Typically 10 to 20% of OD |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 23.0 °C | 2 - 20 % Show Material materials with Dehnung of 2 - 20 % |
Elastizitätsmodul | 23.0 °C | 120 - 138 GPa Show Material materials with Elastizitätsmodul of 120 - 138 GPa |
Streckgrenze Rp 0,2 | 23.0 °C | 340 - 550 MPa Show Material materials with Streckgrenze Rp 0,2 of 340 - 550 MPa |
Zugfestigkeit | 23.0 °C | 440 - 590 MPa Show Material materials with Zugfestigkeit of 440 - 590 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.6E-5 - 1.76E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.76E-5 1/K |
Schmelzpunkt | 1030 - 1040 °C Show Material materials with Schmelzpunkt of 1030 - 1040 °C | |
Spezifische Wärmekapazität | 23.0 °C | 390 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 390 J/(kg·K) |
Wärmeleitfähigkeit | 23.0 °C | 210 - 240 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210 - 240 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Specific Electrical conductivity | 45 - 60 % IACS Show Material materials with Specific Electrical conductivity of 45 - 60 % IACS | |
spezifischer Widerstand | 23.0 °C | 2.9E-6 - 3.8E-6 Ω·m Show Material materials with spezifischer Widerstand of 2.9E-6 - 3.8E-6 Ω·m |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 0 - 0.2 % Show Material materials with Aluminium of 0 - 0.2 % | |
Andere | 0 - 0.5 % Show Material materials with Andere of 0 - 0.5 % | |
Beryllium | 0.2 - 0.6 % Show Material materials with Beryllium of 0.2 - 0.6 % | |
Eisen | 0 - 0.1 % Show Material materials with Eisen of 0 - 0.1 % | |
Kobalt | 0 - 0.3 % Show Material materials with Kobalt of 0 - 0.3 % | |
Kupfer | 95.9 - 98.4 % Show Material materials with Kupfer of 95.9 - 98.4 % | Balance |
Nickel | 1.4 - 2.2 % Show Material materials with Nickel of 1.4 - 2.2 % | |
Silizium | 0 - 0.2 % Show Material materials with Silizium of 0 - 0.2 % |
Technological properties
Property | ||
---|---|---|
Application areas | Typical applications include resistance welding components, and inserts for metal die casting, injection molding and blow molding.,Typical applications include dies casting plunger tips and dies for steel extrusion.,Typical applications include heat exchanger tubing and resistance welding components.,Typical applications include coil springs and formed wire contacts. |