Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 6.0 % Show Material materials with Dehnung of 6.0 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2 | Bar, Tube | A50 |
6.0 - 10.0 % Show Material materials with Dehnung of 6.0 - 10.0 % | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | ||
8.0 % Show Material materials with Dehnung of 8.0 % | T6 | AA Standards, ASTM B221 | A100 | ||
8.5 % Show Material materials with Dehnung of 8.5 % | T6 | ||||
9.0 % Show Material materials with Dehnung of 9.0 % | T6 | BS EN 573-3, BS EN 485-2 | Plate | A50 | |
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T6 | ||||
Härte, Brinell | 84.0 - 91.0 [-] Show Material materials with Härte, Brinell of 84.0 - 91.0 [-] | T6 | BS EN 573-3, BS EN 485-2 | Plate | |
94.0 [-] Show Material materials with Härte, Brinell of 94.0 [-] | T6 | BS EN 573-3, BS EN 485-2 | Sheet | ||
95.0 [-] Show Material materials with Härte, Brinell of 95.0 [-] | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Streckgrenze | 200.0 - 260.0 MPa Show Material materials with Streckgrenze of 200.0 - 260.0 MPa | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | RP02 |
240.0 - 255.0 MPa Show Material materials with Streckgrenze of 240.0 - 255.0 MPa | T6 | BS EN 573-3, BS EN 485-2 | Plate | RP02 | |
260.0 MPa Show Material materials with Streckgrenze of 260.0 MPa | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 485-2 | Sheet | RP02 | |
280.0 MPa Show Material materials with Streckgrenze of 280.0 MPa | T6 | ||||
Zugfestigkeit | 270.0 - 310.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 310.0 MPa | T6 | BS EN 573-3, BS EN 755-2 | Bar, Tube | |
275.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 300.0 MPa | T6 | BS EN 573-3, BS EN 485-2 | Plate | ||
310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 485-2 | Sheet | ||
330.0 MPa Show Material materials with Zugfestigkeit of 330.0 MPa | T6 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T6 | ||||
2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |||
100 °C | 0.000022 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000022 1/K | T6 | unstated value for 20-100°C | |||
Schmelzpunkt | 555.0 °C Show Material materials with Schmelzpunkt of 555.0 °C | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | ||
580.0 °C Show Material materials with Schmelzpunkt of 580.0 °C | T6 | |||||
Spezifische Wärmekapazität | 890.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 890.0 J/(kg·K) | T6 | ||||
Wärmeleitfähigkeit | 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 W/(m·K) | T6 | ||||
180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180.0 W/(m·K) | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Elektrisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium | |||
spezifischer Widerstand | 3.8e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.8e-08 Ω·m | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminium | 95.2 - 98.3 % Show Material materials with Aluminium of 95.2 - 98.3 % | T6 | |||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | Total |
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Eisen | 0.50 % Show Material materials with Eisen of 0.50 % | T6 | AA Standards, ASTM B221 | ||
0.5 % Show Material materials with Eisen of 0.5 % | T6 | BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Mangan | 0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Silizium | 0.7 - 1.3 % Show Material materials with Silizium of 0.7 - 1.3 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | T6 | AA Standards, ASTM B221, BS EN 573-3, BS EN 755-2, BS EN 485-2 | Bar, Tube, Plate, Sheet |
Technological properties
Property | ||
---|---|---|
Application areas | Highly stressed applications, Trusses, Bridges, Cranes, Transport applications, Ore skips, Beer barrels, Milk churns | |
Brazing | Good | |
General machinability | Good | |
Soldering general | Good | |
Welding | 6082 has very good weldability but strength is lowered in the weld zone. When welded to itself, alloy 4043 wire is recommended. If welding 6082 to 7005, then the wire used should be alloy 5356. Gas: Good; Arc: Good; Resistance: Good | |
Workability | Cold: Good |