Abmessung
Property | Value |
---|---|
Durchmesser | 105 - 260 mm Show Supplier Material materials with Durchmesser of 105 - 260 mm |
Mechanisch
Property | Temperature | Value |
---|---|---|
Charpy impact energy, V-notch | -20.0 °C | 32 J Show Supplier Material materials with Charpy impact energy, V-notch of 32 J |
Dehnung | 23.0 °C | 15 % Show Supplier Material materials with Dehnung of 15 % |
Härte, Brinell | 23.0 °C | 341 - 388 [-] Show Supplier Material materials with Härte, Brinell of 341 - 388 [-] |
Streckgrenze Rp 0,2 | 23.0 °C | 1034 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 1034 MPa |
Zugfestigkeit | 23.0 °C | 1138 MPa Show Supplier Material materials with Zugfestigkeit of 1138 MPa |
Chemical properties
Property | Value |
---|---|
Chrom | 0.7 - 0.95 % Show Supplier Material materials with Chrom of 0.7 - 0.95 % |
Eisen | Balance |
Kohlenstoff | 0.28 - 0.33 % Show Supplier Material materials with Kohlenstoff of 0.28 - 0.33 % |
Mangan | 0.75 - 1 % Show Supplier Material materials with Mangan of 0.75 - 1 % |
Molybdän | 0.35 - 0.5 % Show Supplier Material materials with Molybdän of 0.35 - 0.5 % |
Nickel | 1.65 - 2 % Show Supplier Material materials with Nickel of 1.65 - 2 % |
Phosphor | 0.03 % Show Supplier Material materials with Phosphor of 0.03 % |
Schwefel | 0.025 % Show Supplier Material materials with Schwefel of 0.025 % |
Silizium | 0.2 - 0.35 % Show Supplier Material materials with Silizium of 0.2 - 0.35 % |
Vanadium | 0.05 - 0.1 % Show Supplier Material materials with Vanadium of 0.05 - 0.1 % |
Technological properties
Property | ||
---|---|---|
Heat Treatment | Hardened at 840 to 870°C and tempered at 600°C. | |
Welding | Better than AISI 4145, but still challenging. |