Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 1.1 g/cm³ Show Supplier Material materials with Dichte of 1.1 g/cm³ | ASTM D792 |
Abmessung
Mechanisch
Property | Value | Comment |
---|---|---|
Biegefestigkeit | 60.81 MPa Show Supplier Material materials with Biegefestigkeit of 60.81 MPa | ASTM D790 |
Biegemodul | 2.15 GPa Show Supplier Material materials with Biegemodul of 2.15 GPa | ASTM D790 |
Dehnung | 30 % Show Supplier Material materials with Dehnung of 30 % | ASTM D638 |
Streckgrenze | 37.75 MPa Show Supplier Material materials with Streckgrenze of 37.75 MPa | ASTM D638 |
Thermisch
Property | Value | Pressure | Comment |
---|---|---|---|
Vicat-Erweichungstemperatur | 107.0 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 107.0 °C | ASTM D1525 | |
Wärmeformbeständigkeitstemperatur | 90 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 90 °C | 1.8 MPa | ASTM D648, unannealed-annealed condition |
100 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 100 °C | 1.8 MPa | ASTM D648, unannealed-annealed condition |
Technological properties
Property | ||
---|---|---|
Application areas | END-USE PARTS: containers, holders - PROTOTYPES: mechanical parts, architectural models - ELECTRONICS: covers, cases - DECORATIONS: lamps, vases | |
Processing methods | Bed heating required, printing temperature: 250-270°C, bed temperature: 90-110°C |