Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | F | EN 573-3, EN 485, EN 755 | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | F | EN 573-3, EN 755 | A50 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | F | EN 573-3, EN 755 | A100 | |||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Profile, Rod, Tube | A10 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | F | DIN 1725-1 | Forging, Profile, Tube | ||
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | F | EN 573-3, EN 485, EN 755 | |||
20.0 °C | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
Flächenreduzierung | 20.0 °C | 15.0 % Show Material materials with Flächenreduzierung of 15.0 % | F | DIN 1725-1 | Forging | |
20.0 °C | 20.0 % Show Material materials with Flächenreduzierung of 20.0 % | F | DIN 1725-1 | Profile, Tube | ||
Härte, Brinell | 20.0 °C | 65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Tube | |
20.0 °C | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 26.8 GPa Show Material materials with Schubmodule of 26.8 GPa | F | EN 573-3, EN 485, EN 755 | |||
20.0 °C | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
Zugfestigkeit | 245.0 MPa Show Material materials with Zugfestigkeit of 245.0 MPa | F | EN 573-3, EN 485 | |||
250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | F | EN 573-3, EN 485 | ||||
260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | F | EN 573-3, EN 755 | ||||
270.0 MPa Show Material materials with Zugfestigkeit of 270.0 MPa | F | EN 573-3, EN 755 | ||||
20.0 °C | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging | ||
20.0 °C | 270.0 MPa Show Material materials with Zugfestigkeit of 270.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Tube | ||
20.0 °C | 275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Sheet |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | |
-50.0 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
20 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
20 °C | 2.42e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | F | EN 573-3, EN 485, EN 755 | |||
20 °C | 2.6e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
100 °C | 2.42e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
100.0 °C | 2.42e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
200 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | F | EN 573-3, EN 485, EN 755 | |||
200.0 °C | 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
300 °C | 2.6e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
300.0 °C | 2.6e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K | F | EN 573-3, EN 485, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
Max. Betriebstemperatur | -195.0 - 50.0 °C Show Material materials with Max. Betriebstemperatur of -195.0 - 50.0 °C | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Tube | Long | |
150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Schmelzpunkt | 574.0 - 638.0 °C Show Material materials with Schmelzpunkt of 574.0 - 638.0 °C | F | EN 573-3, EN 485, EN 755 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | F | EN 573-3, EN 485, EN 755 | |||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Rod, Sheet, Tube | ||
Wärmeleitfähigkeit | 20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 - 140.0 W/(m·K) | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Rod, Sheet, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 16000000.0 - 19000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 19000000.0 S/m | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Rod, Sheet, Tube |
spezifischer Widerstand | 5.26e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.26e-08 - 6.25e-08 Ω·m | F | EN 573-3, EN 485, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.05 - 0.25 % Show Material materials with Chrom of 0.05 - 0.25 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Tube, Rod, Sheet |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255 | Forging, Profile, Tube, Rod, Sheet |
0.40 % Show Material materials with Eisen of 0.40 % | F | EN 573-3, EN 485, EN 755 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Tube, Rod, Sheet |
Magnesium | 4.0 - 4.9 % Show Material materials with Magnesium of 4.0 - 4.9 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Tube, Rod, Sheet |
Mangan | 0.3 - 1.0 % Show Material materials with Mangan of 0.3 - 1.0 % | F | DIN 1725-1 | Forging, Profile, Tube |
0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Rod, Sheet, Tube | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Tube, Rod, Sheet |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Tube, Rod, Sheet |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | F | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485, EN 755 | Forging, Profile, Tube, Rod, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |