EN 573-3 Grade 3.3547 O

View suppliers (11)
Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMg4,5Mn belongs to the nature-hard aluminum wrought materials, so a strength increase can be achieved only by cold forming, not by a purposeful heat treatment. The material is characterised by good corrosion resistance. It is sea water steady and steady against saline atmosphere. Increasing Mg+Mn content makes the extrusion more difficult, but strength and very low-temperature behaviour improve. The alloy is well weldable. Even in the welding seams strength lie within the range of AlMg5. The alloy AlMg4Mn is standardised as semi-finished material only as sheet metal or strips, thickness: >= 0,35 mm (DIN 1745). Application: rolling shutter and roll gates (sheet metal profiles), in the apparatus engineering for tank bottoms, very low-temperature tanks, heat exchangers and pipings. In the construction of vehicles for superstructures as well as tank and silo trucks, dump truck hollows, buses, bumpers, car body and safety-related parts. In shipbuilding for trunk, superstructures, sail masts and radar equipment

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM,AluKey zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValueConditionRelated StandardsShape

Dichte

2.66 g/cm³

Show Material materials with Dichte of 2.66 g/cm³

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

20.0 °C

2.66 g/cm³

Show Material materials with Dichte of 2.66 g/cm³

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

Mechanisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

125.0 MPa

Show Material materials with Bending Fatigue Strength of 125.0 MPa

O

EN 573-3, EN 1592, EN 485, EN 754, EN 755

Biegewinkel 180°

1.0 °/t

Show Material materials with Biegewinkel 180° of 1.0 °/t

O

EN 573-3, EN 485

1.5 °/t

Show Material materials with Biegewinkel 180° of 1.5 °/t

O

EN 573-3, EN 14286, EN 485

4.0 °/t

Show Material materials with Biegewinkel 180° of 4.0 °/t

O

EN 573-3, EN 14286

Biegewinkel 90°

0.5 °/t

Show Material materials with Biegewinkel 90° of 0.5 °/t

O

EN 573-3, EN 485

1.0 °/t

Show Material materials with Biegewinkel 90° of 1.0 °/t

O

EN 573-3, EN 485

1.5 °/t

Show Material materials with Biegewinkel 90° of 1.5 °/t

O

EN 573-3, EN 485

2.5 °/t

Show Material materials with Biegewinkel 90° of 2.5 °/t

O

EN 573-3, EN 485

Dehnung

9.0 %

Show Material materials with Dehnung of 9.0 %

O

EN 573-3, EN 485

A100

10.0 %

Show Material materials with Dehnung of 10.0 %

O

EN 573-3, EN 485

A100

10.0 %

Show Material materials with Dehnung of 10.0 %

O

EN 573-3, EN 755

A50

11.0 %

Show Material materials with Dehnung of 11.0 %

O

EN 573-3, EN 485

A50

12.0 %

Show Material materials with Dehnung of 12.0 %

O

EN 573-3, EN 485, EN 755

A100

12.0 %

Show Material materials with Dehnung of 12.0 %

O

EN 573-3, EN 485

A50

13.0 %

Show Material materials with Dehnung of 13.0 %

O

EN 573-3, EN 485

A50

14.0 %

Show Material materials with Dehnung of 14.0 %

O

EN 573-3, EN 485

A100

14.0 %

Show Material materials with Dehnung of 14.0 %

O

EN 573-3, EN 754

A50

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3, EN 485

A100

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3, EN 485

A50

16.0 %

Show Material materials with Dehnung of 16.0 %

O

EN 573-3, EN 1592, EN 754

A100

16.0 %

Show Material materials with Dehnung of 16.0 %

O

EN 573-3, EN 485

A50

17.0 %

Show Material materials with Dehnung of 17.0 %

O

EN 573-3, EN 14286

A100

20.0 °C

10.0 %

Show Material materials with Dehnung of 10.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod

A10

20.0 °C

12.0 %

Show Material materials with Dehnung of 12.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod

20.0 °C

12.0 %

Show Material materials with Dehnung of 12.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Tube

A10

20.0 °C

14.0 %

Show Material materials with Dehnung of 14.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Tube, Sheet

20.0 °C

15.0 %

Show Material materials with Dehnung of 15.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Sheet, Strip

A10

20.0 °C

17.0 %

Show Material materials with Dehnung of 17.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Sheet, Strip

20.0 °C

20.0 %

Show Material materials with Dehnung of 20.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

100.0 °C

26.0 %

Show Material materials with Dehnung of 26.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

180.0 °C

43.0 %

Show Material materials with Dehnung of 43.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

240.0 °C

48.0 %

Show Material materials with Dehnung of 48.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

300.0 °C

67.0 %

Show Material materials with Dehnung of 67.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Elastizitätsmodul

71.0 GPa

Show Material materials with Elastizitätsmodul of 71.0 GPa

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

20.0 °C

72.0 GPa

Show Material materials with Elastizitätsmodul of 72.0 GPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

Flächenreduzierung

20.0 °C

15.0 %

Show Material materials with Flächenreduzierung of 15.0 %

O

DIN 1725-1

Sheet

Härte, Brinell

69.0 [-]

Show Material materials with Härte, Brinell of 69.0 [-]

O

EN 573-3, EN 485

70.0 [-]

Show Material materials with Härte, Brinell of 70.0 [-]

O

EN 573-3, EN 485

73.0 [-]

Show Material materials with Härte, Brinell of 73.0 [-]

O

EN 573-3, EN 485

75.0 [-]

Show Material materials with Härte, Brinell of 75.0 [-]

O

EN 573-3, EN 485

20.0 °C

60.0 [-]

Show Material materials with Härte, Brinell of 60.0 [-]

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Tube

20.0 °C

70.0 [-]

Show Material materials with Härte, Brinell of 70.0 [-]

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poissonzahl

0.33 [-]

Show Material materials with Poissonzahl of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Schubmodule

26.8 GPa

Show Material materials with Schubmodule of 26.8 GPa

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

20.0 °C

27.0 GPa

Show Material materials with Schubmodule of 27.0 GPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

Zugfestigkeit

-193.0 °C

495.0 MPa

Show Material materials with Zugfestigkeit of 495.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

-150.0 °C

415.0 MPa

Show Material materials with Zugfestigkeit of 415.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

-105.0 °C

370.0 MPa

Show Material materials with Zugfestigkeit of 370.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

-60.0 °C

355.0 MPa

Show Material materials with Zugfestigkeit of 355.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

-15.0 °C

350.0 MPa

Show Material materials with Zugfestigkeit of 350.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

245.0 MPa

Show Material materials with Zugfestigkeit of 245.0 MPa

O

EN 573-3, EN 485

250.0 MPa

Show Material materials with Zugfestigkeit of 250.0 MPa

O

EN 573-3, EN 485

255.0 MPa

Show Material materials with Zugfestigkeit of 255.0 MPa

O

EN 573-3, EN 485

260.0 MPa

Show Material materials with Zugfestigkeit of 260.0 MPa

O

EN 573-3, EN 485

270.0 - 345.0 MPa

Show Material materials with Zugfestigkeit of 270.0 - 345.0 MPa

O

EN 573-3, EN 485

270.0 - 350.0 MPa

Show Material materials with Zugfestigkeit of 270.0 - 350.0 MPa

O

EN 573-3, EN 754

270.0 MPa

Show Material materials with Zugfestigkeit of 270.0 MPa

O

EN 573-3, EN 755

275.0 MPa

Show Material materials with Zugfestigkeit of 275.0 MPa

O

EN 573-3, EN 1592

290.0 - 370.0 MPa

Show Material materials with Zugfestigkeit of 290.0 - 370.0 MPa

O

EN 573-3, EN 14286

20.0 °C

260.0 MPa

Show Material materials with Zugfestigkeit of 260.0 MPa

O

DIN 1725-1

Sheet

20.0 °C

270.0 MPa

Show Material materials with Zugfestigkeit of 270.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Tube

20.0 °C

275.0 - 350.0 MPa

Show Material materials with Zugfestigkeit of 275.0 - 350.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 485

Sheet, Strip

20.0 °C

321.0 MPa

Show Material materials with Zugfestigkeit of 321.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

20.0 °C

350.0 MPa

Show Material materials with Zugfestigkeit of 350.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

100.0 °C

302.0 MPa

Show Material materials with Zugfestigkeit of 302.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

180.0 °C

209.0 MPa

Show Material materials with Zugfestigkeit of 209.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

240.0 °C

168.0 MPa

Show Material materials with Zugfestigkeit of 168.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

300.0 °C

122.0 MPa

Show Material materials with Zugfestigkeit of 122.0 MPa

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Thermisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Koeffizient der thermischen Ausdehnung

-50 °C

2.23e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

-50.0 °C

2.23e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

20 °C

2.23e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

20 °C

2.42e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

20 °C

2.4999999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

20 °C

2.6e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

100 °C

2.42e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

100.0 °C

2.42e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

200 °C

2.4999999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

200.0 °C

2.5e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

300 °C

2.6e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

300.0 °C

2.6e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755, DIN 1725-1, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

Max. Betriebstemperatur

-195.0 - 50.0 °C

Show Material materials with Max. Betriebstemperatur of -195.0 - 50.0 °C

O

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Strip, Tube

Long

150.0 °C

Show Material materials with Max. Betriebstemperatur of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Schmelzpunkt

574.0 - 638.0 °C

Show Material materials with Schmelzpunkt of 574.0 - 638.0 °C

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

Spezifische Wärmekapazität

900.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K)

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

20.0 °C

900.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K)

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Rod, Sheet, Strip, Tube

Wärmeleitfähigkeit

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 110.0 - 140.0 W/(m·K)

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Sheet, Strip, Tube

Elektrisch

PropertyTemperatureValueConditionRelated StandardsShape

Elektrische Leitfähigkeit

20.0 °C

16000000.0 - 19000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 19000000.0 S/m

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Sheet, Strip, Tube

spezifischer Widerstand

5.26e-08 - 6.25e-08 Ω·m

Show Material materials with spezifischer Widerstand of 5.26e-08 - 6.25e-08 Ω·m

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Chrom

0.05 - 0.25 %

Show Material materials with Chrom of 0.05 - 0.25 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Sheet, Rod, Strip, Tube

Eisen

0.4 %

Show Material materials with Eisen of 0.4 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Sheet, Rod, Strip, Tube

0.40 %

Show Material materials with Eisen of 0.40 %

O

EN 573-3, EN 14286, EN 1592, EN 485, EN 754, EN 755

Kupfer

0.1 %

Show Material materials with Kupfer of 0.1 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Sheet, Rod, Strip, Tube

Magnesium

4.0 - 4.9 %

Show Material materials with Magnesium of 4.0 - 4.9 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Sheet, Rod, Strip, Tube

Mangan

0.3 - 1.0 %

Show Material materials with Mangan of 0.3 - 1.0 %

O

DIN 1725-1

Sheet

0.4 - 1.0 %

Show Material materials with Mangan of 0.4 - 1.0 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Rod, Sheet, Strip, Tube

Silizium

0.4 %

Show Material materials with Silizium of 0.4 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Sheet, Rod, Strip, Tube

Titan

0.15 %

Show Material materials with Titan of 0.15 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Sheet, Rod, Strip, Tube

Zink

0.25 %

Show Material materials with Zink of 0.25 %

O

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 14286, EN 1592, EN 485, EN 754, EN 755

Sheet, Rod, Strip, Tube

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)