Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | |||
Biegewinkel 90° | 2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | T6 | EN 573-3, EN 485 | |||
3.5 °/t Show Material materials with Biegewinkel 90° of 3.5 °/t | T6 | EN 573-3, EN 485 | ||||
4.5 °/t Show Material materials with Biegewinkel 90° of 4.5 °/t | T6 | EN 573-3, EN 485 | ||||
6.0 °/t Show Material materials with Biegewinkel 90° of 6.0 °/t | T6 | EN 573-3, EN 485 | ||||
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | T6 | EN 573-3, EN 485 | A100 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | T6 | EN 573-3, EN 1386 | A50 | |||
3.0 % Show Material materials with Dehnung of 3.0 % | T6 | EN 573-3, EN 1386 | A50 | |||
4.0 % Show Material materials with Dehnung of 4.0 % | T6 | EN 573-3, EN 485 | A100 | |||
4.0 % Show Material materials with Dehnung of 4.0 % | T6 | EN 573-3, EN 1386 | A50 | |||
5.0 % Show Material materials with Dehnung of 5.0 % | T6 | EN 573-3, EN 586 | A100 | |||
6.0 % Show Material materials with Dehnung of 6.0 % | T6 | EN 573-3, EN 1386, EN 485, EN 755 | A100 | |||
6.0 % Show Material materials with Dehnung of 6.0 % | T6 | EN 573-3, EN 1386, EN 485, EN 755 | A50 | |||
7.0 % Show Material materials with Dehnung of 7.0 % | T6 | EN 573-3, EN 485 | A100 | |||
7.0 % Show Material materials with Dehnung of 7.0 % | T6 | EN 573-3, EN 485, EN 754 | A50 | |||
8.0 % Show Material materials with Dehnung of 8.0 % | T6 | EN 573-3, EN 485, EN 754, EN 755 | A100 | |||
8.0 % Show Material materials with Dehnung of 8.0 % | T6 | EN 573-3, EN 755 | A50 | |||
9.0 % Show Material materials with Dehnung of 9.0 % | T6 | EN 573-3, EN 485, EN 754 | A50 | |||
10.0 % Show Material materials with Dehnung of 10.0 % | T6 | EN 573-3, EN 1301 | ||||
10.0 % Show Material materials with Dehnung of 10.0 % | T6 | EN 573-3, EN 754, EN 755 | A100 | |||
10.0 % Show Material materials with Dehnung of 10.0 % | T6 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A100 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A10 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | T6 | DIN 1725-1 | Tube | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | |||
20.0 °C | 68.0 - 73.0 GPa Show Material materials with Elastizitätsmodul of 68.0 - 73.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire | ||
Härte, Brinell | 83.0 [-] Show Material materials with Härte, Brinell of 83.0 [-] | T6 | EN 573-3, EN 485 | |||
84.0 [-] Show Material materials with Härte, Brinell of 84.0 [-] | T6 | EN 573-3, EN 485 | ||||
89.0 [-] Show Material materials with Härte, Brinell of 89.0 [-] | T6 | EN 573-3, EN 485 | ||||
90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T6 | EN 573-3, EN 586 | ||||
91.0 [-] Show Material materials with Härte, Brinell of 91.0 [-] | T6 | EN 573-3, EN 485 | ||||
94.0 [-] Show Material materials with Härte, Brinell of 94.0 [-] | T6 | EN 573-3, EN 485 | ||||
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | ||
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Scherfestigkeit | 20.0 °C | 180.0 MPa Show Material materials with Scherfestigkeit of 180.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | |
Schubmodule | 26.4 GPa Show Material materials with Schubmodule of 26.4 GPa | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | |||
20.0 °C | 26.0 - 27.0 GPa Show Material materials with Schubmodule of 26.0 - 27.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire | ||
Streckgrenze | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | T6 | EN 573-3, EN 755 | RP02 | ||
220.0 MPa Show Material materials with Streckgrenze of 220.0 MPa | T6 | EN 573-3, EN 485 | RP02 | |||
230.0 MPa Show Material materials with Streckgrenze of 230.0 MPa | T6 | EN 573-3, EN 485 | RP02 | |||
240.0 MPa Show Material materials with Streckgrenze of 240.0 MPa | T6 | EN 573-3, EN 485, EN 754, EN 755 | RP02 | |||
250.0 MPa Show Material materials with Streckgrenze of 250.0 MPa | T6 | EN 573-3, EN 586, EN 755 | RP02 | |||
255.0 MPa Show Material materials with Streckgrenze of 255.0 MPa | T6 | EN 573-3, EN 485, EN 754 | RP02 | |||
260.0 MPa Show Material materials with Streckgrenze of 260.0 MPa | T6 | EN 573-3, EN 1386, EN 485, EN 755 | RP02 | |||
270.0 MPa Show Material materials with Streckgrenze of 270.0 MPa | T6 | EN 573-3, EN 1301 | RP02 | |||
20.0 °C | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire, Forging | RP02 | |
20.0 °C | 220.0 MPa Show Material materials with Streckgrenze of 220.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | RP02 | |
20.0 °C | 250.0 MPa Show Material materials with Streckgrenze of 250.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | RP02 | |
20.0 °C | 260.0 MPa Show Material materials with Streckgrenze of 260.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | RP02 | |
20.0 °C | 270.0 MPa Show Material materials with Streckgrenze of 270.0 MPa | T6 | DIN 1725-1 | Tube | ||
Zugfestigkeit | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6 | EN 573-3, EN 485 | |||
270.0 MPa Show Material materials with Zugfestigkeit of 270.0 MPa | T6 | EN 573-3, EN 755 | ||||
275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | T6 | EN 573-3, EN 485 | ||||
280.0 MPa Show Material materials with Zugfestigkeit of 280.0 MPa | T6 | EN 573-3, EN 755 | ||||
290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T6 | EN 573-3, EN 586, EN 755 | ||||
295.0 MPa Show Material materials with Zugfestigkeit of 295.0 MPa | T6 | EN 573-3, EN 485, EN 755 | ||||
300.0 MPa Show Material materials with Zugfestigkeit of 300.0 MPa | T6 | EN 573-3, EN 1301, EN 485 | ||||
310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T6 | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||||
20.0 °C | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
20.0 °C | 275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire, Forging | ||
20.0 °C | 290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
20.0 °C | 310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
20.0 °C | 320.0 MPa Show Material materials with Zugfestigkeit of 320.0 MPa | T6 | DIN 1725-1 | Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | ||
Schmelzpunkt | 585.0 - 650.0 °C Show Material materials with Schmelzpunkt of 585.0 - 650.0 °C | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | ||
Spezifische Wärmekapazität | 896.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 896.0 J/(kg·K) | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | ||
Wärmeleitfähigkeit | 20.0 °C | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Forging, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 24000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 32000000.0 S/m | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Forging, Wire |
spezifischer Widerstand | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-08 - 4.17e-08 Ω·m | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Forging, Wire |
0.3 % Show Material materials with Chrom of 0.3 % | T6 | DIN 1725-1 | Tube | |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | T6 | DIN 1725-1 | Tube |
0.5 % Show Material materials with Eisen of 0.5 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire | |
0.50 % Show Material materials with Eisen of 0.50 % | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | ||
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | T6 | DIN 1725-1 | Tube |
0.1 % Show Material materials with Kupfer of 0.1 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Forging, Wire | |
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Tube, Forging, Wire |
Mangan | 0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Tube, Forging, Wire |
Silizium | 0.7 - 1.3 % Show Material materials with Silizium of 0.7 - 1.3 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Forging, Wire |
0.75 - 1.3 % Show Material materials with Silizium of 0.75 - 1.3 % | T6 | DIN 1725-1 | Tube | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Tube, Forging, Wire |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | T6 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 485, EN 586, EN 754, EN 755 | Tube, Forging, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |