Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
Elastizitätsmodul | 20.0 °C | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | |
Härte, Brinell | 20.0 °C | 130.0 [-] Show Material materials with Härte, Brinell of 130.0 [-] | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse |
20.0 °C | 130.0 [-] Show Material materials with Härte, Brinell of 130.0 [-] | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 150.0 [-] Show Material materials with Härte, Brinell of 150.0 [-] | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse | |
Kompressionsmodul | 20.0 °C | 72.5 GPa Show Material materials with Kompressionsmodul of 72.5 GPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | |
Plane-Strain Fracture Toughnes | 20.0 °C | 24.0 - 41.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 41.1 MPa·√m | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | |
20.0 °C | 24.0 - 33.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 33.2 MPa·√m | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 24.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 MPa·√m | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 33.2 - 41.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.2 - 41.1 MPa·√m | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 33.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.2 MPa·√m | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 41.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 41.1 MPa·√m | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Schubmodule | 26.4 - 27.1 GPa Show Material materials with Schubmodule of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Zugfestigkeit | 20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse |
20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 480.0 MPa Show Material materials with Zugfestigkeit of 480.0 MPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | ||
20.0 °C | 490.0 MPa Show Material materials with Zugfestigkeit of 490.0 MPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse | |
20.0 °C | 520.0 MPa Show Material materials with Zugfestigkeit of 520.0 MPa | T73511 | WL 3.4364-1, DIN 1725-1 | Profile | Transverse |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.1e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Schmelzpunkt | 465.0 - 655.0 °C Show Material materials with Schmelzpunkt of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Spezifische Wärmekapazität | 795.0 - 1050.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Wärmeleitfähigkeit | 121.0 - 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.18 - 0.28 % Show Material materials with Chrom of 0.18 - 0.28 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Eisen | 0.5 Show Material materials with Eisen of 0.5 | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Kupfer | 1.2 - 2.0 % Show Material materials with Kupfer of 1.2 - 2.0 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Magnesium | 2.1 - 2.9 % Show Material materials with Magnesium of 2.1 - 2.9 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Mangan | 0.3 Show Material materials with Mangan of 0.3 | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Silizium | 0.4 Show Material materials with Silizium of 0.4 | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Titan | 0.2 Show Material materials with Titan of 0.2 | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Zink | 5.1 - 6.1 % Show Material materials with Zink of 5.1 - 6.1 % | T73511 | WL 3.4364-1, DIN 1725-1 | Profile |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |