Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
4.0 °/t Show Material materials with Biegewinkel 90° of 4.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | |
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat, Rod, Tube | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | O | EN 573-3 | Flat | A50 Transverse | |
Elastizitätsmodul | 72.5 GPa Show Material materials with Elastizitätsmodul of 72.5 GPa | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 65.0 - 73.5 GPa Show Material materials with Elastizitätsmodul of 65.0 - 73.5 GPa | O | EN 573-3 | Rod, Flat, Tube | ||
Härte, Brinell | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | O | EN 573-3 | Flat | Transverse | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 27.2 GPa Show Material materials with Schubmodule of 27.2 GPa | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 26.0 - 28.5 GPa Show Material materials with Schubmodule of 26.0 - 28.5 GPa | O | EN 573-3 | Rod, Flat, Tube | ||
Zugfestigkeit | 150.0 - 220.0 MPa Show Material materials with Zugfestigkeit of 150.0 - 220.0 MPa | O | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Tube, Bar | ||
225.0 MPa Show Material materials with Zugfestigkeit of 225.0 MPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | |||
250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 225.0 MPa Show Material materials with Zugfestigkeit of 225.0 MPa | O | EN 573-3 | Flat | ||
20.0 °C | 225.0 MPa Show Material materials with Zugfestigkeit of 225.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 436.0 MPa Show Material materials with Zugfestigkeit of 436.0 MPa | O | EN 573-3 | |||
100.0 °C | 394.0 MPa Show Material materials with Zugfestigkeit of 394.0 MPa | O | EN 573-3 | |||
150.0 °C | 281.0 MPa Show Material materials with Zugfestigkeit of 281.0 MPa | O | EN 573-3 | |||
200.0 °C | 155.0 MPa Show Material materials with Zugfestigkeit of 155.0 MPa | O | EN 573-3 | |||
250.0 °C | 84.0 MPa Show Material materials with Zugfestigkeit of 84.0 MPa | O | EN 573-3 | |||
300.0 °C | 46.0 MPa Show Material materials with Zugfestigkeit of 46.0 MPa | O | EN 573-3 | |||
370.0 °C | 32.0 MPa Show Material materials with Zugfestigkeit of 32.0 MPa | O | EN 573-3 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
100 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Schmelzpunkt | 512.0 - 650.0 °C Show Material materials with Schmelzpunkt of 512.0 - 650.0 °C | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Spezifische Wärmekapazität | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 921.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube |
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 200.0 W/(m·K) | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 18000000.0 - 28000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 28000000.0 S/m | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
spezifischer Widerstand | 3.57e-08 - 5.56e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.57e-08 - 5.56e-08 Ω·m | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Flat, Rod, Tube, Strip, Sheet, Plate, Bar |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | O | EN 573-3 | Flat, Rod, Tube |
0.70 % Show Material materials with Eisen of 0.70 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 3.5 - 4.5 % Show Material materials with Kupfer of 3.5 - 4.5 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Flat, Rod, Tube, Strip, Sheet, Plate, Bar |
Magnesium | 0.4 - 1.0 % Show Material materials with Magnesium of 0.4 - 1.0 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Flat, Rod, Tube, Strip, Sheet, Plate, Bar |
Mangan | 0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Flat, Rod, Tube, Strip, Sheet, Plate, Bar |
Silizium | 0.2 - 0.8 % Show Material materials with Silizium of 0.2 - 0.8 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Flat, Rod, Tube, Strip, Sheet, Plate, Bar |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | O | EN 573-3, EN 1715-3, EN 485, EN 754, EN 755 | Flat, Rod, Tube, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: sufficient | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) acceptable (O) / acceptable (O) |