Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.75 - 2.84 g/cm³ Show Material materials with Dichte of 2.75 - 2.84 g/cm³ | Typical for Wrought 2000 Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | -269.0 °C | 82.0 GPa Show Material materials with Elastizitätsmodul of 82.0 GPa | T851 | EN 573-3 | ||
-195.0 °C | 78.6 GPa Show Material materials with Elastizitätsmodul of 78.6 GPa | T851 | EN 573-3 | |||
27.0 °C | 70.8 GPa Show Material materials with Elastizitätsmodul of 70.8 GPa | T851 | EN 573-3 | |||
Plane-Strain Fracture Toughnes | 20.0 °C | 32.6 - 36.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.6 - 36.6 MPa·√m | T851 | EN 573-3 | ||
20.0 °C | 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.6 MPa·√m | T851 | EN 573-3 | |||
20.0 °C | 36.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.0 - 39.0 MPa·√m | T851 | EN 573-3 | Sheet | ||
20.0 °C | 36.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.0 MPa·√m | T851 | EN 573-3 | Sheet | ||
20.0 °C | 36.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.6 MPa·√m | T851 | EN 573-3 | |||
20.0 °C | 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 39.0 MPa·√m | T851 | EN 573-3 | Sheet | ||
Poissonzahl | -269.0 °C | 0.341 [-] Show Material materials with Poissonzahl of 0.341 [-] | T851 | EN 573-3 | ||
-195.0 °C | 0.355 [-] Show Material materials with Poissonzahl of 0.355 [-] | T851 | EN 573-3 | |||
27.0 °C | 0.313 [-] Show Material materials with Poissonzahl of 0.313 [-] | T851 | EN 573-3 | |||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Streckgrenze | -269.0 °C | 461.3 MPa Show Material materials with Streckgrenze of 461.3 MPa | T851 | EN 573-3 | RP02 | |
-195.0 °C | 413.7 MPa Show Material materials with Streckgrenze of 413.7 MPa | T851 | EN 573-3 | RP02 | ||
20.0 °C | 435.0 MPa Show Material materials with Streckgrenze of 435.0 MPa | T851 | EN 573-3 | Sheet | ||
27.0 °C | 361.2 MPa Show Material materials with Streckgrenze of 361.2 MPa | T851 | EN 573-3 | RP02 | ||
Zugfestigkeit | -269.0 °C | 663.9 MPa Show Material materials with Zugfestigkeit of 663.9 MPa | T851 | EN 573-3 | ||
-195.0 °C | 563.9 MPa Show Material materials with Zugfestigkeit of 563.9 MPa | T851 | EN 573-3 | |||
27.0 °C | 470.2 MPa Show Material materials with Zugfestigkeit of 470.2 MPa | T851 | EN 573-3 |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Schmelzpunkt | 500.0 - 650.0 °C Show Material materials with Schmelzpunkt of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Wärmeleitfähigkeit | 112.0 - 251.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
spezifischer Widerstand | 3.4e-08 - 6e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.3 Show Material materials with Eisen of 0.3 | T851 | EN 573-3 | Sheet |
Kupfer | 5.8 - 6.8 % Show Material materials with Kupfer of 5.8 - 6.8 % | T851 | EN 573-3 | Sheet |
Magnesium | 0.02 Show Material materials with Magnesium of 0.02 | T851 | EN 573-3 | Sheet |
Mangan | 0.2 - 0.4 % Show Material materials with Mangan of 0.2 - 0.4 % | T851 | EN 573-3 | Sheet |
Silizium | 0.2 Show Material materials with Silizium of 0.2 | T851 | EN 573-3 | Sheet |
Titan | 0.02 - 0.1 % Show Material materials with Titan of 0.02 - 0.1 % | T851 | EN 573-3 | Sheet |
Vanadium | 0.05 - 0.15 % Show Material materials with Vanadium of 0.05 - 0.15 % | T851 | EN 573-3 | Sheet |
Zink | 0.1 Show Material materials with Zink of 0.1 | T851 | EN 573-3 | Sheet |
Zirkonium | 0.1 - 0.25 % Show Material materials with Zirkonium of 0.1 - 0.25 % | T851 | EN 573-3 | Sheet |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |