General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Densidad of 2.68 - 2.69 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
Dureza Brinell | 20.0 °C | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | F | EN 573-3 | Profile, Rod, Tube | |
Elongación | 13.0 % Show Material materials with Elongación of 13.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | |
15.0 % Show Material materials with Elongación of 15.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | F | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | F | EN 573-3 | Profile, Rod, Tube | ||
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.3 - 27.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 165.0 MPa Show Material materials with Resistencia a la tracción of 165.0 MPa | F | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
180.0 - 250.0 MPa Show Material materials with Resistencia a la tracción of 180.0 - 250.0 MPa | F | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 165.0 MPa Show Material materials with Resistencia a la tracción of 165.0 MPa | F | EN 573-3 | Flat | ||
20.0 °C | 165.0 MPa Show Material materials with Resistencia a la tracción of 165.0 MPa | F | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | F | EN 573-3 | Profile, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 901.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Calor específico of 901.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Coeficiente de dilatación térmica | -50.0 °C | 2.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.21e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
200 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.57e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 138.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 - 150.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | ||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Temperatura de fusión of 607.0 - 649.0 °C | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-08 - 4.95e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-08 - 5.2e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 - 5.2e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | F | EN 573-3 | Profile, Rod, Flat, Tube, Plate |
0.40 % Show Material materials with Hierro of 0.40 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | F | EN 573-3, EN 1386, EN 1715-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Plate, Strip, Sheet, Foil, Wire, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |