General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3 | Sheet, Rod, Flat, Tube | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Densidad of 2.68 - 2.69 g/cm³ | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H111 | EN 573-3 | Rod, Flat, Tube |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H111 | EN 573-3 | Rod, Flat, Tube | |
Dureza Brinell | 46.0 [-] Show Material materials with Dureza Brinell of 46.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 46.0 - 47.0 [-] Show Material materials with Dureza Brinell of 46.0 - 47.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 46.0 [-] Show Material materials with Dureza Brinell of 46.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H111 | EN 573-3 | Rod, Tube, Flat | ||
Dureza Brinell (HBW) | 47 [-] Show Material materials with Dureza Brinell (HBW) of 47 [-] | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
Elongación | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | |
12 % Show Material materials with Elongación of 12 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
18.0 % Show Material materials with Elongación of 18.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
19.0 % Show Material materials with Elongación of 19.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongación of 20.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | H111 | EN 573-3 | Rod, Tube | ||
Límite elástico | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | |
65 MPa Show Material materials with Límite elástico of 65 MPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
20.0 °C | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | H111 | EN 573-3 | Rod, Tube, Flat | RP02 | |
20.0 °C | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | H111 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | H111 | EN 573-3 | Rod, Tube | RP02 | |
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.3 - 27.0 GPa | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | H111 | EN 573-3 | Rod, Flat, Tube | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 573-3 | Sheet, Rod, Flat, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 165.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 215.0 MPa | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 165.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 215.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | H111 | EN 573-3 | Rod | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 230.0 MPa | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 215.0 MPa | H111 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 215.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Ángulo de flexión a 90° | 0 °/t Show Material materials with Ángulo de flexión a 90° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 901.0 J/(kg·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Calor específico of 901.0 J/(kg·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
Coeficiente de dilatación térmica | -50.0 °C | 2.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.21e-05 1/K | H111 | EN 573-3 | Rod, Flat, Tube | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | 20-100°C | |
200 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.57e-05 1/K | H111 | EN 573-3 | Rod, Flat, Tube | ||
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 138.0 W/(m·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 - 150.0 W/(m·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 W/(m·K) | H111 | EN 573-3 | Rod, Flat, Tube | ||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Temperatura de fusión of 607.0 - 649.0 °C | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
4.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.9e-08 Ω·m | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-08 - 4.95e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-08 - 5.2e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 - 5.2e-08 Ω·m | H111 | EN 573-3 | Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.1 % Show Material materials with Cobre of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H111 | EN 573-3 | Rod, Flat, Tube |
0.40 % Show Material materials with Hierro of 0.40 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
0.4 % Show Material materials with Hierro of 0.4 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.1 % Show Material materials with Manganeso of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.25 % Show Material materials with Silicona of 0.25 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H111 | EN 573-3, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Wire, Bar |
0.1 % Show Material materials with Zinc of 0.1 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |