General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Elongación | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | |
10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3 | Flat | Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3 | Flat | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3 | Sheet, Flat | ||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Módulo elástico | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 360.0 - 440.0 MPa Show Material materials with Resistencia a la tracción of 360.0 - 440.0 MPa | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
370.0 - 440.0 MPa Show Material materials with Resistencia a la tracción of 370.0 - 440.0 MPa | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 360.0 - 440.0 MPa Show Material materials with Resistencia a la tracción of 360.0 - 440.0 MPa | H321 | EN 573-3 | Flat | Transverse | |
20.0 °C | 360.0 MPa Show Material materials with Resistencia a la tracción of 360.0 MPa | H321 | EN 573-3 | Sheet | ||
20.0 °C | 370.0 - 440.0 MPa Show Material materials with Resistencia a la tracción of 370.0 - 440.0 MPa | H321 | EN 573-3 | Flat | Transverse | |
20.0 °C | 370.0 MPa Show Material materials with Resistencia a la tracción of 370.0 MPa | H321 | EN 573-3 | Flat | ||
Ángulo de flexión a 180° | 3.0 °/t Show Material materials with Ángulo de flexión a 180° of 3.0 °/t | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
6.0 °/t Show Material materials with Ángulo de flexión a 180° of 6.0 °/t | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Coeficiente de dilatación térmica | 2.2e-05 - 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Conductividad térmica | 112.0 - 205.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Temperatura de fusión | 560.0 - 655.0 °C Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 31000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
Resistividad eléctrica | 3.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Circonio | 0.05 - 0.25 % Show Material materials with Circonio of 0.05 - 0.25 % | H321 | EN 573-3 | Flat, Sheet |
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | H321 | EN 573-3, EN 485, EN 13195 | Flat, Sheet, Strip, Plate |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | H321 | EN 573-3 | Flat, Sheet |
0.3 % Show Material materials with Cromo of 0.3 % | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate | |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | H321 | EN 573-3 | Flat, Sheet |
0.50 % Show Material materials with Hierro of 0.50 % | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate | |
Magnesio | 3.5 - 4.5 % Show Material materials with Magnesio of 3.5 - 4.5 % | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate |
5.0 - 6.0 % Show Material materials with Magnesio of 5.0 - 6.0 % | H321 | EN 573-3 | Flat, Sheet | |
Manganeso | 0.4 - 0.8 % Show Material materials with Manganeso of 0.4 - 0.8 % | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate |
0.6 - 1.2 % Show Material materials with Manganeso of 0.6 - 1.2 % | H321 | EN 573-3 | Flat, Sheet | |
Silicona | 0.45 % Show Material materials with Silicona of 0.45 % | H321 | EN 573-3, EN 485, EN 13195 | Flat, Sheet, Strip, Plate |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate |
0.2 % Show Material materials with Titanio of 0.2 % | H321 | EN 573-3 | Flat, Sheet | |
Zinc | 0.4 - 0.9 % Show Material materials with Zinc of 0.4 - 0.9 % | H321 | EN 573-3 | Flat, Sheet |
0.4 - 0.8 % Show Material materials with Zinc of 0.4 - 0.8 % | H321 | EN 573-3, EN 485, EN 13195 | Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |