General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 2.64 - 2.66 g/cm³ Show Material materials with Densidad of 2.64 - 2.66 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 2.64 g/cm³ Show Material materials with Densidad of 2.64 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
Dureza Brinell | 20.0 °C | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | F | EN 573-3 | Profile, Tube, Rod | |
Elongación | 10.0 % Show Material materials with Elongación of 10.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | |
12.0 % Show Material materials with Elongación of 12.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | F | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | F | EN 573-3 | Profile, Tube, Rod | ||
Módulo de cizallamiento | 26.8 GPa Show Material materials with Módulo de cizallamiento of 26.8 GPa | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 26.8 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.8 - 27.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 26.8 GPa Show Material materials with Módulo de cizallamiento of 26.8 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | |
71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 70.0 - 71.0 GPa Show Material materials with Módulo elástico of 70.0 - 71.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 245.0 MPa Show Material materials with Resistencia a la tracción of 245.0 MPa | F | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | F | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
20.0 °C | 245.0 MPa Show Material materials with Resistencia a la tracción of 245.0 MPa | F | EN 573-3 | Sheet | ||
20.0 °C | 245.0 MPa Show Material materials with Resistencia a la tracción of 245.0 MPa | F | EN 573-3 | Flat | Transverse | |
20.0 °C | 250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | F | EN 573-3 | Flat | ||
20.0 °C | 250.0 MPa Show Material materials with Resistencia a la tracción of 250.0 MPa | F | EN 573-3 | Flat | Transverse | |
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | F | EN 573-3 | Rod | ||
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | F | EN 573-3 | Profile, Tube, Rod |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 899.0 - 900.0 J/(kg·K) Show Material materials with Calor específico of 899.0 - 900.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 899.0 J/(kg·K) Show Material materials with Calor específico of 899.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Coeficiente de dilatación térmica | -50 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | |
-50.0 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.42e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.42e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20 °C | 2.6e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
100 °C | 2.42e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.42e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
100.0 °C | 2.42e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.42e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
200 °C | 2.4999999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4999999999999998e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
200.0 °C | 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
300 °C | 2.6e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 2.6e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.6e-05 1/K | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | ||
Conductividad térmica | 20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 140.0 W/(m·K) | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat | |
20.0 °C | 110.0 - 117.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 117.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 117.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 117.0 - 140.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 117.0 W/(m·K) Show Material materials with Conductividad térmica of 117.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Temperatura de fusión | 574.0 - 638.0 °C Show Material materials with Temperatura de fusión of 574.0 - 638.0 °C | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
Temperatura máx. de funcionamiento | -195.0 - 50.0 °C Show Material materials with Temperatura máx. de funcionamiento of -195.0 - 50.0 °C | F | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | Long | |
150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 16000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 19000000.0 S/m | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile, Rod, Flat |
Resistividad eléctrica | 5.26e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 - 6.25e-08 Ω·m | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 5.2e-08 - 6e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-08 - 6e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 5.2e-08 - 6.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-08 - 6.2e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 6e-08 Ω·m Show Material materials with Resistividad eléctrica of 6e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 6e-08 - 6.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 6e-08 - 6.2e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | F | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
0.40 % Show Material materials with Hierro of 0.40 % | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Magnesio | 4.0 - 4.9 % Show Material materials with Magnesio of 4.0 - 4.9 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | F | EN 573-3, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |