General
Property | Value | Comment |
---|---|---|
Densidad | 2.65 - 2.7 g/cm³ Show Material materials with Densidad of 2.65 - 2.7 g/cm³ | Typical for Wrought 5000 Series Aluminium |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||
Módulo elástico | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | Typical for Wrought 5000 Series Aluminium | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Resistencia a la tracción | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 | |
275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | H112 | AA Standards, ASTM B209, ASTM B247 |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Coeficiente de dilatación térmica | 2.2e-05 - 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Conductividad térmica | 112.0 - 205.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Temperatura de fusión | 560.0 - 655.0 °C Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 31000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
Resistividad eléctrica | 3.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Magnesio | 4.0 - 4.9 % Show Material materials with Magnesio of 4.0 - 4.9 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B247, ASTM B345 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: kein Schadensfall im Betrieb und bei Labortests (O, H321, H116), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (H111), general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor | |
Workability | general (condition): acceptable (O), poor(H321, H116, H111) |