General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H321 | EN 573-3 | Flat | |
20.0 °C | 2.66 - 2.67 g/cm³ Show Material materials with Densidad of 2.66 - 2.67 g/cm³ | H321 | EN 573-3 | Flat | |
20.0 °C | 2.67 g/cm³ Show Material materials with Densidad of 2.67 g/cm³ | H321 | EN 573-3 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H321 | EN 573-3 | Flat | |
Dureza Brinell | 81.0 [-] Show Material materials with Dureza Brinell of 81.0 [-] | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 81.0 [-] Show Material materials with Dureza Brinell of 81.0 [-] | H321 | EN 573-3 | Flat | ||
Elongación | 8.0 % Show Material materials with Elongación of 8.0 % | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | |
9.0 % Show Material materials with Elongación of 9.0 % | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
9.0 % Show Material materials with Elongación of 9.0 % | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H321 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H321 | EN 573-3 | Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H321 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H321 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H321 | EN 573-3 | Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H321 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H321 | EN 573-3 | Flat | A50 | |
Módulo de cizallamiento | 26.7 GPa Show Material materials with Módulo de cizallamiento of 26.7 GPa | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 26.7 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.7 - 27.0 GPa | H321 | EN 573-3 | Flat | ||
20.0 °C | 26.7 GPa Show Material materials with Módulo de cizallamiento of 26.7 GPa | H321 | EN 573-3 | Flat | ||
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | H321 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 275.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 360.0 MPa | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 275.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 360.0 MPa | H321 | EN 573-3 | Flat | Transverse | |
20.0 °C | 275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | H321 | EN 573-3 | Flat | ||
Ángulo de flexión a 180° | 2.0 °/t Show Material materials with Ángulo de flexión a 180° of 2.0 °/t | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Ángulo de flexión a 90° | 2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
3.5 °/t Show Material materials with Ángulo de flexión a 90° of 3.5 °/t | H321 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H321 | EN 573-3 | Flat | ||
Coeficiente de dilatación térmica | -50 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | |
-50.0 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
20 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
200 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
200.0 °C | 2.47e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.47e-05 1/K | H321 | EN 573-3 | Flat | ||
300 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
300.0 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
Conductividad térmica | 126 W/(m·K) Show Material materials with Conductividad térmica of 126 W/(m·K) | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 120.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 140.0 W/(m·K) | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | ||
20.0 °C | 120.0 - 126.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 126.0 W/(m·K) | H321 | EN 573-3 | Flat | ||
20.0 °C | 126.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 126.0 - 140.0 W/(m·K) | H321 | EN 573-3 | Flat | ||
20.0 °C | 126.0 W/(m·K) Show Material materials with Conductividad térmica of 126.0 W/(m·K) | H321 | EN 573-3 | Flat | ||
Temperatura de fusión | 585.0 - 641.0 °C Show Material materials with Temperatura de fusión of 585.0 - 641.0 °C | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
585.0 - 640.0 °C Show Material materials with Temperatura de fusión of 585.0 - 640.0 °C | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 18000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 S/m | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 17000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 19000000.0 S/m | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat | |
Resistividad eléctrica | 5.26e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 - 5.88e-08 Ω·m | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-08 Ω·m | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 5.2e-08 - 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-08 - 5.6e-08 Ω·m | H321 | EN 573-3 | Flat | |
20.0 °C | 5.2e-08 - 5.8e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-08 - 5.8e-08 Ω·m | H321 | EN 573-3 | Flat | |
20.0 °C | 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.6e-08 Ω·m | H321 | EN 573-3 | Flat | |
20.0 °C | 5.6e-08 - 5.8e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.6e-08 - 5.8e-08 Ω·m | H321 | EN 573-3 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | H321 | EN 573-3 | Flat |
0.50 % Show Material materials with Hierro of 0.50 % | H321 | EN 573-3, EN 13195, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
Magnesio | 3.5 - 4.5 % Show Material materials with Magnesio of 3.5 - 4.5 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Manganeso | 0.2 - 0.7 % Show Material materials with Manganeso of 0.2 - 0.7 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H321 | EN 573-3, EN 13195, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |