General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Strip, Sheet, Plate |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | H111 | EN 573-3, EN 13195 | Strip, Sheet, Plate | ||
75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
76.0 [-] Show Material materials with Dureza Brinell of 76.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
85.0 [-] Show Material materials with Dureza Brinell of 85.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 75.0 - 85.0 [-] Show Material materials with Dureza Brinell of 75.0 - 85.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 75.0 - 80.0 [-] Show Material materials with Dureza Brinell of 75.0 - 80.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 75.0 - 76.0 [-] Show Material materials with Dureza Brinell of 75.0 - 76.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 76.0 - 85.0 [-] Show Material materials with Dureza Brinell of 76.0 - 85.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 76.0 - 80.0 [-] Show Material materials with Dureza Brinell of 76.0 - 80.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 76.0 [-] Show Material materials with Dureza Brinell of 76.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 80.0 - 85.0 [-] Show Material materials with Dureza Brinell of 80.0 - 85.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 85.0 [-] Show Material materials with Dureza Brinell of 85.0 [-] | H111 | EN 573-3 | Flat | ||
Elongación | 11.0 % Show Material materials with Elongación of 11.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | |
12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | H111 | EN 573-3, EN 13195 | Strip, Sheet, Plate | |||
17.0 % Show Material materials with Elongación of 17.0 % | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate | A100 | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3 | Sheet | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H111 | EN 573-3 | Sheet | ||
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Módulo elástico | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | H111 | EN 573-3, EN 13195 | Strip, Sheet, Plate | |||
290.0 - 370.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 370.0 MPa | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate | |||
20.0 °C | 270.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 270.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 270.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 270.0 - 355.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 275.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 275.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 275.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 355.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 285.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 285.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 285.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 285.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 285.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 285.0 - 355.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 290.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 290.0 - 355.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 290.0 - 360.0 MPa Show Material materials with Resistencia a la tracción of 290.0 - 360.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Flat | ||
Resistencia al cizallamiento | 20.0 °C | 75.0 - 80.0 MPa Show Material materials with Resistencia al cizallamiento of 75.0 - 80.0 MPa | H111 | EN 573-3 | Sheet | |
20.0 °C | 75.0 - 76.0 MPa Show Material materials with Resistencia al cizallamiento of 75.0 - 76.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 75.0 MPa Show Material materials with Resistencia al cizallamiento of 75.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 76.0 - 80.0 MPa Show Material materials with Resistencia al cizallamiento of 76.0 - 80.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 76.0 MPa Show Material materials with Resistencia al cizallamiento of 76.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 80.0 MPa Show Material materials with Resistencia al cizallamiento of 80.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 85.0 MPa Show Material materials with Resistencia al cizallamiento of 85.0 MPa | H111 | EN 573-3 | Flat | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | H111 | EN 573-3, EN 14286, EN 485 | Strip, Sheet, Plate | |||
4.0 °/t Show Material materials with Ángulo de flexión a 180° of 4.0 °/t | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 879.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Coeficiente de dilatación térmica | 2.2e-05 - 2.5e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Conductividad térmica | 112.0 - 205.0 W/(m·K) Show Material materials with Conductividad térmica of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Temperatura de fusión | 560.0 - 655.0 °C Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 31000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
Resistividad eléctrica | 3.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Circonio | 0.2 % Show Material materials with Circonio of 0.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Cobre | 0.2 % Show Material materials with Cobre of 0.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Hierro | 0.25 % Show Material materials with Hierro of 0.25 % | H111 | EN 573-3 | Flat, Sheet |
0.25 % Show Material materials with Hierro of 0.25 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Strip, Sheet, Plate | |
Magnesio | 4.0 - 5.2 % Show Material materials with Magnesio of 4.0 - 5.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Manganeso | 0.7 - 1.0 % Show Material materials with Manganeso of 0.7 - 1.0 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Zinc | 0.4 % Show Material materials with Zinc of 0.4 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |