General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 2.66 - 2.68 g/cm³ Show Material materials with Densidad of 2.66 - 2.68 g/cm³ | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
Dureza Brinell | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | H112 | EN 573-3, EN 586 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
52.0 [-] Show Material materials with Dureza Brinell of 52.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
62.0 [-] Show Material materials with Dureza Brinell of 62.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20.0 °C | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H112 | EN 573-3 | Profile, Tube, Rod | ||
20.0 °C | 50.0 [-] Show Material materials with Dureza Brinell of 50.0 [-] | H112 | EN 573-3 | Forging | ||
20.0 °C | 52.0 - 62.0 [-] Show Material materials with Dureza Brinell of 52.0 - 62.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 52.0 - 58.0 [-] Show Material materials with Dureza Brinell of 52.0 - 58.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 52.0 [-] Show Material materials with Dureza Brinell of 52.0 [-] | H112 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 58.0 - 62.0 [-] Show Material materials with Dureza Brinell of 58.0 - 62.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 62.0 [-] Show Material materials with Dureza Brinell of 62.0 [-] | H112 | EN 573-3 | Flat | ||
Elongación | 10.0 % Show Material materials with Elongación of 10.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | |
12.0 % Show Material materials with Elongación of 12.0 % | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
13.0 % Show Material materials with Elongación of 13.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
14.0 % Show Material materials with Elongación of 14.0 % | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
14.0 % Show Material materials with Elongación of 14.0 % | H112 | EN 573-3, EN 485, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
15.0 % Show Material materials with Elongación of 15.0 % | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
15.0 % Show Material materials with Elongación of 15.0 % | H112 | EN 573-3, EN 586 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H112 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H112 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H112 | EN 573-3 | Profile, Rod, Tube, Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H112 | EN 573-3 | Sheet | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | H112 | EN 573-3 | Rod | ||
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H112 | EN 573-3 | Rod, Sheet, Tube, Profile | ||
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | H112 | EN 573-3 | Rod, Tube, Profile, Forging | ||
Módulo de cizallamiento | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 26.5 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.5 - 27.0 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
20.0 °C | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
Módulo elástico | -270 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
70.5 GPa Show Material materials with Módulo elástico of 70.5 GPa | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 70.0 - 70.5 GPa Show Material materials with Módulo elástico of 70.0 - 70.5 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
20.0 °C | 70.5 GPa Show Material materials with Módulo elástico of 70.5 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
300 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H112 | EN 573-3, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | H112 | EN 573-3 | Rod, Tube, Profile, Forging | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Resistencia a la tracción of 190.0 - 240.0 MPa | H112 | EN 573-3 | Transverse | ||
20.0 °C | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | H112 | EN 573-3 | Sheet, Flat | ||
Resistencia al choque, ensayo Charpy entallado | 30.0 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 30.0 kJ/m² | H112 | EN 573-3 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 20.0 °C | 897.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 897.0 - 963.0 J/(kg·K) | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 897.0 J/(kg·K) Show Material materials with Calor específico of 897.0 J/(kg·K) | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
20.0 °C | 963.0 J/(kg·K) Show Material materials with Calor específico of 963.0 J/(kg·K) | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
Coeficiente de dilatación térmica | 20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3899999999999998e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
100.0 °C | 2.39e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.39e-05 1/K | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
Conductividad térmica | 20.0 °C | 132.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 132.0 - 160.0 W/(m·K) | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 132.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 132.0 - 140.0 W/(m·K) | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
20.0 °C | 132.0 W/(m·K) Show Material materials with Conductividad térmica of 132.0 W/(m·K) | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | ||
20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 - 160.0 W/(m·K) | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat | ||
Temperatura de fusión | 610.0 - 640.0 °C Show Material materials with Temperatura de fusión of 610.0 - 640.0 °C | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 23000000.0 S/m | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Profile, Rod, Flat |
Resistividad eléctrica | 4.35e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 - 5e-08 Ω·m | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
20.0 °C | 4.3e-08 - 5.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-08 - 5.3e-08 Ω·m | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 4.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-08 - 5e-08 Ω·m | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 5e-08 - 5.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 - 5.3e-08 Ω·m | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube | |
20.0 °C | 5.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.3e-08 Ω·m | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H112 | EN 573-3 | Profile, Forging, Rod, Sheet, Flat, Tube |
0.40 % Show Material materials with Hierro of 0.40 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
Magnesio | 2.6 - 3.6 % Show Material materials with Magnesio of 2.6 - 3.6 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H112 | EN 573-3, EN 13195, EN 485, EN 586, EN 603, EN 755 | Profile, Forging, Rod, Sheet, Flat, Tube, Strip, Plate, Wire, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |