General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | O | AA Standards, ASTM B221, ASTM B241 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Dureza Brinell | 43.0 [-] Show Material materials with Dureza Brinell of 43.0 [-] | O | AA Standards | |
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | AA Standards, ASTM B221, ASTM B241 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Resistencia a la tracción | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | O | AA Standards | |
200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | O | AA Standards, ASTM B221, ASTM B241 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | |||
Coeficiente de dilatación térmica | 20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | AA Standards, ASTM B221, ASTM B241 | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | AA Standards, ASTM B221, ASTM B241 | ||
Conductividad térmica | 146.0 - 155.0 W/(m·K) Show Material materials with Conductividad térmica of 146.0 - 155.0 W/(m·K) | O | AA Standards, ASTM B221, ASTM B241 | ||
Temperatura de fusión | 560.0 - 645.0 °C Show Material materials with Temperatura de fusión of 560.0 - 645.0 °C | O | AA Standards, ASTM B221, ASTM B241 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 21000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 - 23000000.0 S/m | O | AA Standards, ASTM B221, ASTM B241 |
Resistividad eléctrica | 4.35e-08 - 4.76e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 - 4.76e-08 Ω·m | O | AA Standards, ASTM B221, ASTM B241 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 0.7 - 1.2 % Show Material materials with Cobre of 0.7 - 1.2 % | O | AA Standards, ASTM B221, ASTM B241 |
Cromo | 0.4 % Show Material materials with Cromo of 0.4 % | O | AA Standards, ASTM B221, ASTM B241 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | O | AA Standards, ASTM B221, ASTM B241 |
Magnesio | 0.8 - 1.4 % Show Material materials with Magnesio of 0.8 - 1.4 % | O | AA Standards, ASTM B221, ASTM B241 |
Manganeso | 0.6 - 1.1 % Show Material materials with Manganeso of 0.6 - 1.1 % | O | AA Standards, ASTM B221, ASTM B241 |
Silicona | 0.9 - 1.8 % Show Material materials with Silicona of 0.9 - 1.8 % | O | AA Standards, ASTM B221, ASTM B241 |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | O | AA Standards, ASTM B221, ASTM B241 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | AA Standards, ASTM B221, ASTM B241 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O), no damage during operation, limited damage during laboratory tests, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), sufficient (T4, T4510, T4511), good to acceptable (T6, T6510, T6511) | |
Workability | general (condition): acceptable (O), poor(T4, T4510, T4511, T6, T6510, T6511) |