General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.75 g/cm³ Show Material materials with Densidad of 2.75 g/cm³ | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | |
20.0 °C | 2.75 g/cm³ Show Material materials with Densidad of 2.75 g/cm³ | T6 | EN 573-3 | Profile, Rod, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 105.0 [-] Show Material materials with Dureza Brinell of 105.0 [-] | T6 | EN 573-3 | Profile, Rod, Tube | |
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | A100 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3 | Profile, Rod, Tube | ||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T6 | EN 573-3, EN 755 | Rod, Tube | ||
310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | |||
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T6 | EN 573-3 | Rod | ||
20.0 °C | 310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T6 | EN 573-3 | Profile, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | |
100.0 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T6 | EN 573-3 | Profile, Rod, Tube | ||
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | ||
Conductividad térmica | 170.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 220.0 W/(m·K) | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | ||
20.0 °C | 163.0 - 186.0 W/(m·K) Show Material materials with Conductividad térmica of 163.0 - 186.0 W/(m·K) | T6 | EN 573-3 | Profile, Rod, Tube | ||
Temperatura de fusión | 585.0 - 650.0 °C Show Material materials with Temperatura de fusión of 585.0 - 650.0 °C | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 24000000.0 - 32000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 32000000.0 S/m | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | |
20.0 °C | 24000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 28000000.0 S/m | T6 | EN 573-3 | Profile, Rod, Tube | |
Resistividad eléctrica | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.13e-08 - 4.17e-08 Ω·m | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bismuto | 0.7 % Show Material materials with Bismuto of 0.7 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T6 | EN 573-3 | Profile, Rod, Tube |
0.50 % Show Material materials with Hierro of 0.50 % | T6 | EN 573-3, EN 754, EN 755 | Rod, Tube | |
Magnesio | 0.6 - 1.2 % Show Material materials with Magnesio of 0.6 - 1.2 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Plomo | 0.4 - 2.0 % Show Material materials with Plomo of 0.4 - 2.0 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Silicona | 0.6 - 1.4 % Show Material materials with Silicona of 0.6 - 1.4 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Zinc | 0.3 % Show Material materials with Zinc of 0.3 % | T6 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable / - |