General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 25.0 MPa Show Material materials with Bending Fatigue Strength of 25.0 MPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
35.0 MPa Show Material materials with Bending Fatigue Strength of 35.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Dureza Brinell | 34.0 [-] Show Material materials with Dureza Brinell of 34.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 30.0 [-] Show Material materials with Dureza Brinell of 30.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 34.0 [-] Show Material materials with Dureza Brinell of 34.0 [-] | H14 | EN 573-3 | Flat | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Foil | A50 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3 | Wire | A100 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3 | Rod, Tube, Flat | ||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 25.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 25.0 - 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 25.9 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 25.9 - 26.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
-195.0 °C | 78.4 GPa Show Material materials with Módulo elástico of 78.4 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
-85.0 °C | 73.5 GPa Show Material materials with Módulo elástico of 73.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
-30.0 °C | 71.4 GPa Show Material materials with Módulo elástico of 71.4 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Módulo elástico of 60.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.0 - 68.6 GPa Show Material materials with Módulo elástico of 68.0 - 68.6 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.6 GPa Show Material materials with Módulo elástico of 68.6 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.0 - 66.5 GPa Show Material materials with Módulo elástico of 66.0 - 66.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.5 GPa Show Material materials with Módulo elástico of 66.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 56.0 - 57.0 GPa Show Material materials with Módulo elástico of 56.0 - 57.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 56.0 GPa Show Material materials with Módulo elástico of 56.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 100.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 100.0 - 135.0 MPa | H14 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 100.0 MPa Show Material materials with Resistencia a la tracción of 100.0 MPa | H14 | EN 573-3 | Wire | ||
20.0 °C | 105.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 145.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 105.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 145.0 MPa | H14 | EN 573-3, EN 485, EN 683 | Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 899.0 - 900.0 J/(kg·K) Show Material materials with Calor específico of 899.0 - 900.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 899.0 J/(kg·K) Show Material materials with Calor específico of 899.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Coeficiente de dilatación térmica | -50 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
20 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Conductividad térmica | 20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 220.0 W/(m·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
20.0 °C | 210.0 - 229.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 229.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 220.0 - 229.0 W/(m·K) Show Material materials with Conductividad térmica of 220.0 - 229.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 229.0 W/(m·K) Show Material materials with Conductividad térmica of 229.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Temperatura de fusión | 646.0 - 657.0 °C Show Material materials with Temperatura de fusión of 646.0 - 657.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 34000000.0 - 36000000.0 S/m Show Material materials with Conductividad eléctrica of 34000000.0 - 36000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Conductividad eléctrica of 34800000.0 - 36000000.0 S/m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Resistividad eléctrica | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.78e-08 - 2.94e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.8e-08 - 2.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.8e-08 - 2.9e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 2.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.5 % Show Material materials with Aluminio of 99.5 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Boro | 0.05 Show Material materials with Boro of 0.05 | H14 | EN 573-3 | Flat |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Cromo | 0.01 Show Material materials with Cromo of 0.01 | H14 | EN 573-3 | Flat |
Galio | 0.03 Show Material materials with Galio of 0.03 | H14 | EN 573-3 | Flat |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H14 | EN 573-3 | Flat, Rod, Foil, Tube, Wire |
0.40 % Show Material materials with Hierro of 0.40 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Magnesio | 0.03 % Show Material materials with Magnesio of 0.03 % | H14 | EN 573-3 | Flat |
0.05 % Show Material materials with Magnesio of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Manganeso | 0.01 % Show Material materials with Manganeso of 0.01 % | H14 | EN 573-3 | Flat |
0.05 % Show Material materials with Manganeso of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Níquel | 0.03 Show Material materials with Níquel of 0.03 | H14 | EN 573-3 | Flat |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | H14 | EN 573-3 | Flat |
0.25 % Show Material materials with Silicona of 0.25 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | H14 | EN 573-3 | Flat |
0.05 % Show Material materials with Titanio of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Vanadio | 0.03 Show Material materials with Vanadio of 0.03 | H14 | EN 573-3 | Flat |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | H14 | EN 573-3 | Flat |
0.07 % Show Material materials with Zinc of 0.07 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |