General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.83 g/cm³ Show Material materials with Densidad of 2.83 g/cm³ | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||
Resistencia a la tracción | 565.0 MPa Show Material materials with Resistencia a la tracción of 565.0 MPa | T6 | AA Standards, ASTM B221, ASTM B241 | |
570.0 MPa Show Material materials with Resistencia a la tracción of 570.0 MPa | T6 | AA Standards, ASTM B209 | ||
580.0 MPa Show Material materials with Resistencia a la tracción of 580.0 MPa | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 | ||
595.0 MPa Show Material materials with Resistencia a la tracción of 595.0 MPa | T6 | AA Standards, ASTM B221 | ||
600.0 MPa Show Material materials with Resistencia a la tracción of 600.0 MPa | T6 | AA Standards, ASTM B221, ASTM B241 | ||
605.0 MPa Show Material materials with Resistencia a la tracción of 605.0 MPa | T6 | AA Standards |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium | |||
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 | ||
Conductividad térmica | 126 W/(m·K) Show Material materials with Conductividad térmica of 126 W/(m·K) | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 | ||
Temperatura de fusión | 475.0 - 630.0 °C Show Material materials with Temperatura de fusión of 475.0 - 630.0 °C | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 18000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 S/m | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Resistividad eléctrica | 5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-08 Ω·m | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 1.6 - 2.4 % Show Material materials with Cobre of 1.6 - 2.4 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Cromo | 0.18 - 0.28 % Show Material materials with Cromo of 0.18 - 0.28 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Magnesio | 2.4 - 3.1 % Show Material materials with Magnesio of 2.4 - 3.1 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Manganeso | 0.3 % Show Material materials with Manganeso of 0.3 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Zinc | 6.3 - 7.3 % Show Material materials with Zinc of 6.3 - 7.3 % | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B316 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: good to acceptable | |
Workability | general (condition): not suitable |