Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | T66 | EN 573-3 | Profile, Rod, Tube | |
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T66 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | T66 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T66 | EN 573-3 | Rod, Tube, Profile | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T66 | EN 573-3 | Rod, Tube, Profile | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 25.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 GPa | T66 | EN 573-3 | Profile, Rod, Tube | ||
Módulo elástico | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 67.0 GPa Show Material materials with Módulo elástico of 67.0 GPa | T66 | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | T66 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | T66 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | T66 | EN 573-3 | Profile | ||
20.0 °C | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | T66 | EN 573-3 | Rod, Tube, Profile |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 898.0 J/(kg·K) Show Material materials with Calor específico of 898.0 J/(kg·K) | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Coeficiente de dilatación térmica | -50 °C | 2.18e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar |
20 °C | 2.18e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.18e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.56e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.56e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
200 °C | 2.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.45e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
300 °C | 2.56e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.56e-05 1/K | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Conductividad térmica | 200.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 200.0 - 220.0 W/(m·K) | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 220.0 W/(m·K) Show Material materials with Conductividad térmica of 220.0 W/(m·K) | T66 | EN 573-3 | Profile, Rod, Tube | |
Temperatura de fusión | 585.0 - 650.0 °C Show Material materials with Temperatura de fusión of 585.0 - 650.0 °C | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 28000000.0 - 31000000.0 S/m Show Material materials with Conductividad eléctrica of 28000000.0 - 31000000.0 S/m | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 30000000.0 - 32000000.0 S/m Show Material materials with Conductividad eléctrica of 30000000.0 - 32000000.0 S/m | T66 | EN 573-3 | Profile, Rod, Tube | |
Resistividad eléctrica | 3.23e-08 - 3.57e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.23e-08 - 3.57e-08 Ω·m | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Cromo | 0.05 % Show Material materials with Cromo of 0.05 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Hierro | 0.1 - 0.3 % Show Material materials with Hierro of 0.1 - 0.3 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Magnesio | 0.35 - 0.6 % Show Material materials with Magnesio of 0.35 - 0.6 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Silicona | 0.3 - 0.6 % Show Material materials with Silicona of 0.3 - 0.6 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Zinc | 0.15 % Show Material materials with Zinc of 0.15 % | T66 | EN 573-3, EN 12020, EN 13195, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: EQ: sehr gut, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / good, friction soldering: very good, soft brazing with flux: good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / -, Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) - / good (O) |