General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Dureza Brinell | 40.0 [-] Show Material materials with Dureza Brinell of 40.0 [-] | F | EN 573-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | |
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Resistencia a la tracción | 120.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 200.0 MPa | F | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | |
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
Conductividad térmica | 155.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 155.0 - 180.0 W/(m·K) | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
170.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 200.0 W/(m·K) | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
Temperatura de fusión | 580.0 - 640.0 °C Show Material materials with Temperatura de fusión of 580.0 - 640.0 °C | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
580.0 - 650.0 °C Show Material materials with Temperatura de fusión of 580.0 - 650.0 °C | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 22000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 30000000.0 S/m | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
23000000.0 - 27000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 27000000.0 S/m | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Resistividad eléctrica | 3.33e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.33e-08 - 4.55e-08 Ω·m | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
3.7e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.7e-08 - 4.35e-08 Ω·m | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.15 - 0.4 % Show Material materials with Cobre of 0.15 - 0.4 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Cromo | 0.04 - 0.35 % Show Material materials with Cromo of 0.04 - 0.35 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Hierro | 0.70 % Show Material materials with Hierro of 0.70 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Magnesio | 0.8 - 1.2 % Show Material materials with Magnesio of 0.8 - 1.2 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Silicona | 0.4 - 0.8 % Show Material materials with Silicona of 0.4 - 0.8 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | F | EN 573-3, EN 1715-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |