General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | ||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 110.0 - 160.0 MPa Show Material materials with Resistencia a la tracción of 110.0 - 160.0 MPa | H14 | EN 573-3 | Foil | |
20.0 °C | 120.0 - 170.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 170.0 MPa | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | ||
Conductividad térmica | 193.0 - 218.0 W/(m·K) Show Material materials with Conductividad térmica of 193.0 - 218.0 W/(m·K) | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | ||
Temperatura de fusión | 615.0 - 655.0 °C Show Material materials with Temperatura de fusión of 615.0 - 655.0 °C | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 29000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 29000000.0 - 34000000.0 S/m | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar |
Resistividad eléctrica | 2.94e-08 - 3.45e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.45e-08 Ω·m | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Hierro | 0.35 % Show Material materials with Hierro of 0.35 % | H14 | EN 573-3 | Foil |
0.35 % Show Material materials with Hierro of 0.35 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Bar | |
Magnesio | 0.45 - 0.9 % Show Material materials with Magnesio of 0.45 - 0.9 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Silicona | 0.2 - 0.6 % Show Material materials with Silicona of 0.2 - 0.6 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): acceptable to poor / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Excellent workability. |