General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 55.0 MPa Show Material materials with Bending Fatigue Strength of 55.0 MPa | O | AA Standards | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Dureza Brinell | 25.0 [-] Show Material materials with Dureza Brinell of 25.0 [-] | O | AA Standards, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Elongación | 16.0 % Show Material materials with Elongación of 16.0 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | A50 |
16.0 % Show Material materials with Elongación of 16.0 % | O | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A100 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Resistencia a la tracción | 90.0 MPa Show Material materials with Resistencia a la tracción of 90.0 MPa | O | AA Standards | ||
130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
Conductividad térmica | 193.0 - 218.0 W/(m·K) Show Material materials with Conductividad térmica of 193.0 - 218.0 W/(m·K) | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
200.0 W/(m·K) Show Material materials with Conductividad térmica of 200.0 W/(m·K) | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |||
Temperatura de fusión | 600.0 °C Show Material materials with Temperatura de fusión of 600.0 °C | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
615.0 - 655.0 °C Show Material materials with Temperatura de fusión of 615.0 - 655.0 °C | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 29000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 29000000.0 - 34000000.0 S/m | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
Resistividad eléctrica | 2.94e-08 - 3.45e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.45e-08 Ω·m | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
3.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.5e-08 Ω·m | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Hierro | 0.35 % Show Material materials with Hierro of 0.35 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
0.35 % Show Material materials with Hierro of 0.35 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Magnesio | 0.45 - 0.9 % Show Material materials with Magnesio of 0.45 - 0.9 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | Total |
Silicona | 0.2 - 0.6 % Show Material materials with Silicona of 0.2 - 0.6 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Technological properties
Property | ||
---|---|---|
Application areas | - 6063 Architectural, applications, Extrusions, Window frames, Doors, Shop fittings, Irrigation tubing, In balustrading the rails and posts are normally in the T6 temper and formed elbows and bends are T4. T4 temper 6063 aluminium is also finding applications in hydroformed tube for chassis. - 6063A 6063A is used in the same applications as 6063. It is also used in: Road transport Rail transport Extreme sports equipment | |
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (T1, T4), sufficient (T5, T452, T6, T83, T831, T832) | |
Soldering general | Good | |
Welding | 6063 is suitable for all conventional welding methods. Welding wire generally should be alloy 5183 or alloy 4043. When maximum electrical conductivity is required use alloy 4043. For strength and conductivity use alloy 5346 and increase the size of the weld to compensate for the lower conductivity. Gas: Excellent; Arc:Excellent; Resistance:Excellent. | |
Workability | general (condition): acceptable (T1, T4, T5, T452), poor(T6, T83, T831, T832) |