General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | H42 | EN 573-3 | Sheet, Strip | |
20.0 °C | 2.71 - 2.72 g/cm³ Show Material materials with Densidad of 2.71 - 2.72 g/cm³ | H42 | EN 573-3 | Sheet, Strip | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | H42 | EN 573-3 | Sheet, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H42 | EN 573-3 | Sheet, Strip | |
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.0 GPa | H42 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 24.0 - 25.9 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 25.9 GPa | H42 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 25.9 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 25.9 - 26.0 GPa | H42 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H42 | EN 573-3 | Sheet, Strip | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | H42 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | H42 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Módulo elástico of 65.0 - 69.0 GPa | H42 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H42 | EN 573-3 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 85.0 - 125.0 MPa Show Material materials with Resistencia a la tracción of 85.0 - 125.0 MPa | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 90.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 90.0 - 135.0 MPa | H42 | EN 573-3 | Sheet, Strip | Transverse | |
20.0 °C | 90.0 - 135.0 MPa Show Material materials with Resistencia a la tracción of 90.0 - 135.0 MPa | H42 | EN 573-3 | Sheet, Strip |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 898.0 J/(kg·K) Show Material materials with Calor específico of 898.0 J/(kg·K) | H42 | EN 573-3 | Sheet, Strip |
Coeficiente de dilatación térmica | -50 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | H42 | EN 573-3 | Sheet, Strip | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | H42 | EN 573-3 | Sheet, Strip | |
Conductividad térmica | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 210.0 W/(m·K) | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
20.0 °C | 205.0 - 225.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 225.0 W/(m·K) | H42 | EN 573-3 | Sheet, Strip | |
20.0 °C | 210.0 - 225.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 225.0 W/(m·K) | H42 | EN 573-3 | Sheet, Strip | |
20.0 °C | 225.0 W/(m·K) Show Material materials with Conductividad térmica of 225.0 W/(m·K) | H42 | EN 573-3 | Sheet, Strip | |
Temperatura de fusión | 644.0 - 657.0 °C Show Material materials with Temperatura de fusión of 644.0 - 657.0 °C | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 33000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 - 34000000.0 S/m | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Conductividad eléctrica of 34400000.0 - 35500000.0 S/m | H42 | EN 573-3 | Sheet, Strip | |
Resistividad eléctrica | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.94e-08 - 3.03e-08 Ω·m | H42 | EN 573-3, EN 1396 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.95e-08 Ω·m | H42 | EN 573-3 | Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.0 % Show Material materials with Aluminio of 99.0 % | H42 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H42 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | H42 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | H42 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H42 | EN 573-3, EN 1396 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |