General
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 83.0 [-] Show Material materials with Dureza Brinell of 83.0 [-] | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
84.0 [-] Show Material materials with Dureza Brinell of 84.0 [-] | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
89.0 [-] Show Material materials with Dureza Brinell of 89.0 [-] | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
91.0 [-] Show Material materials with Dureza Brinell of 91.0 [-] | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
94.0 [-] Show Material materials with Dureza Brinell of 94.0 [-] | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20.0 °C | 83.0 [-] Show Material materials with Dureza Brinell of 83.0 [-] | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 83.0 - 89.0 [-] Show Material materials with Dureza Brinell of 83.0 - 89.0 [-] | T62 | EN 573-3 | Sheet | ||
20.0 °C | 83.0 - 84.0 [-] Show Material materials with Dureza Brinell of 83.0 - 84.0 [-] | T62 | EN 573-3 | Sheet | ||
20.0 °C | 83.0 [-] Show Material materials with Dureza Brinell of 83.0 [-] | T62 | EN 573-3 | Sheet | ||
20.0 °C | 84.0 - 94.0 [-] Show Material materials with Dureza Brinell of 84.0 - 94.0 [-] | T62 | EN 573-3 | Flat | ||
20.0 °C | 84.0 - 91.0 [-] Show Material materials with Dureza Brinell of 84.0 - 91.0 [-] | T62 | EN 573-3 | Flat | ||
20.0 °C | 84.0 - 89.0 [-] Show Material materials with Dureza Brinell of 84.0 - 89.0 [-] | T62 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 84.0 [-] Show Material materials with Dureza Brinell of 84.0 [-] | T62 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 89.0 - 94.0 [-] Show Material materials with Dureza Brinell of 89.0 - 94.0 [-] | T62 | EN 573-3 | Flat | ||
20.0 °C | 89.0 - 91.0 [-] Show Material materials with Dureza Brinell of 89.0 - 91.0 [-] | T62 | EN 573-3 | Flat | ||
20.0 °C | 89.0 [-] Show Material materials with Dureza Brinell of 89.0 [-] | T62 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 91.0 - 94.0 [-] Show Material materials with Dureza Brinell of 91.0 - 94.0 [-] | T62 | EN 573-3 | Flat | ||
20.0 °C | 91.0 [-] Show Material materials with Dureza Brinell of 91.0 [-] | T62 | EN 573-3 | Flat | ||
20.0 °C | 94.0 [-] Show Material materials with Dureza Brinell of 94.0 [-] | T62 | EN 573-3 | Flat | ||
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | |
4.0 % Show Material materials with Elongación of 4.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
8.0 % Show Material materials with Elongación of 8.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
9.0 % Show Material materials with Elongación of 9.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T62 | EN 573-3 | Sheet | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T62 | EN 573-3 | Sheet | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T62 | EN 573-3 | Sheet | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T62 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T62 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T62 | EN 573-3 | Profile, Sheet | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T62 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T62 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T62 | EN 573-3 | Flat | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T62 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | T62 | EN 573-3 | Flat | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T62 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T62 | EN 573-3 | Flat | A50 | |
Módulo de cizallamiento | 26.4 GPa Show Material materials with Módulo de cizallamiento of 26.4 GPa | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 26.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.0 GPa | T62 | EN 573-3 | Profile, Flat, Sheet | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 68.0 - 73.0 GPa Show Material materials with Módulo elástico of 68.0 - 73.0 GPa | T62 | EN 573-3 | Profile, Flat, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 255.0 MPa Show Material materials with Resistencia a la tracción of 255.0 MPa | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
295.0 MPa Show Material materials with Resistencia a la tracción of 295.0 MPa | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T62 | EN 573-3 | Sheet | ||
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | T62 | EN 573-3 | Sheet | ||
20.0 °C | 275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 295.0 MPa Show Material materials with Resistencia a la tracción of 295.0 MPa | T62 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 295.0 MPa Show Material materials with Resistencia a la tracción of 295.0 MPa | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | T62 | EN 573-3 | Flat | ||
20.0 °C | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | T62 | EN 573-3 | Flat | Transverse | |
20.0 °C | 310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T62 | EN 573-3 | Profile, Flat | ||
20.0 °C | 310.0 MPa Show Material materials with Resistencia a la tracción of 310.0 MPa | T62 | EN 573-3 | Flat | Transverse | |
Ángulo de flexión a 90° | 2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
3.5 °/t Show Material materials with Ángulo de flexión a 90° of 3.5 °/t | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
4.5 °/t Show Material materials with Ángulo de flexión a 90° of 4.5 °/t | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
6.0 °/t Show Material materials with Ángulo de flexión a 90° of 6.0 °/t | T62 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 896.0 J/(kg·K) Show Material materials with Calor específico of 896.0 J/(kg·K) | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
Coeficiente de dilatación térmica | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
Conductividad térmica | 20.0 °C | 170.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 220.0 W/(m·K) | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Temperatura de fusión | 585.0 - 650.0 °C Show Material materials with Temperatura de fusión of 585.0 - 650.0 °C | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 24000000.0 - 32000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 32000000.0 S/m | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Resistividad eléctrica | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.13e-08 - 4.17e-08 Ω·m | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Cromo | 0.25 % Show Material materials with Cromo of 0.25 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T62 | EN 573-3 | Profile, Flat, Sheet |
0.50 % Show Material materials with Hierro of 0.50 % | T62 | EN 573-3, EN 485, EN 603 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
Magnesio | 0.6 - 1.2 % Show Material materials with Magnesio of 0.6 - 1.2 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Manganeso | 0.4 - 1.0 % Show Material materials with Manganeso of 0.4 - 1.0 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Silicona | 0.7 - 1.3 % Show Material materials with Silicona of 0.7 - 1.3 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | T62 | EN 573-3, EN 485, EN 603 | Profile, Flat, Sheet, Strip, Plate, Wire, Forging, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |