General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Dureza Brinell | 20.0 °C | 170.0 [-] Show Material materials with Dureza Brinell of 170.0 [-] | T6510 | EN 573-3 | Tube, Profile, Rod | |
Elongación | 3.0 % Show Material materials with Elongación of 3.0 % | T6510 | EN 573-3, EN 755 | Rod, Tube | A100 | |
4.0 % Show Material materials with Elongación of 4.0 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T6510 | EN 573-3, EN 754 | Rod, Tube | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T6510 | EN 573-3, EN 755 | Rod, Tube | A100 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T6510 | EN 573-3, EN 754 | Rod, Tube | A100 | ||
7.0 % Show Material materials with Elongación of 7.0 % | T6510 | EN 573-3, EN 754 | Rod, Tube | A100 | ||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T6510 | EN 573-3 | Rod | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T6510 | EN 573-3 | Tube, Profile, Rod | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T6510 | EN 573-3 | Tube | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T6510 | EN 573-3 | Tube, Profile, Rod | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6510 | EN 573-3 | Tube | ||
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | T6510 | EN 573-3 | Tube | ||
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Módulo elástico | 69.0 - 72.0 GPa Show Material materials with Módulo elástico of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Resistencia a la tracción | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
520.0 MPa Show Material materials with Resistencia a la tracción of 520.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
560.0 MPa Show Material materials with Resistencia a la tracción of 560.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
590.0 MPa Show Material materials with Resistencia a la tracción of 590.0 MPa | T6510 | EN 573-3, EN 754 | Rod, Tube | |||
610.0 MPa Show Material materials with Resistencia a la tracción of 610.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
20.0 °C | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 520.0 MPa Show Material materials with Resistencia a la tracción of 520.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 560.0 MPa Show Material materials with Resistencia a la tracción of 560.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 590.0 MPa Show Material materials with Resistencia a la tracción of 590.0 MPa | T6510 | EN 573-3 | Tube | ||
20.0 °C | 610.0 MPa Show Material materials with Resistencia a la tracción of 610.0 MPa | T6510 | EN 573-3 | Tube, Profile, Rod |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Coeficiente de dilatación térmica | 2.1e-05 - 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Conductividad térmica | 121.0 - 170.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Temperatura de fusión | 465.0 - 655.0 °C Show Material materials with Temperatura de fusión of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
Resistividad eléctrica | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 1.2 - 1.9 % Show Material materials with Cobre of 1.2 - 1.9 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T6510 | EN 573-3 | Rod, Tube, Profile |
0.50 % Show Material materials with Hierro of 0.50 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube | |
Magnesio | 2.1 - 3.1 % Show Material materials with Magnesio of 2.1 - 3.1 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Zinc | 7.2 - 8.4 % Show Material materials with Zinc of 7.2 - 8.4 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |