General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube |
Medidas
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Espesor | 0.2 mm Show Material materials with Espesor of 0.2 mm | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | 0.2 mm | Coil, Sheet, Strip |
3 mm Show Material materials with Espesor of 3 mm | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | 3 mm | Coil, Sheet, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | |
Dureza Brinell | 20.0 [-] Show Material materials with Dureza Brinell of 20.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 20.0 [-] Show Material materials with Dureza Brinell of 20.0 [-] | H111 | EN 573-3 | Flat, Rod, Tube | ||
Dureza Brinell (HBW) | 20 [-] Show Material materials with Dureza Brinell (HBW) of 20 [-] | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | ||
Elongación | 20 % Show Material materials with Elongación of 20 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | A50 | |
20.0 % Show Material materials with Elongación of 20.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
22.0 % Show Material materials with Elongación of 22.0 % | H111 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
23.0 % Show Material materials with Elongación of 23.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
25.0 % Show Material materials with Elongación of 25.0 % | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
25.0 % Show Material materials with Elongación of 25.0 % | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
26.0 % Show Material materials with Elongación of 26.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
29.0 % Show Material materials with Elongación of 29.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
32.0 % Show Material materials with Elongación of 32.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
35.0 % Show Material materials with Elongación of 35.0 % | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
35.0 % Show Material materials with Elongación of 35.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 22.0 % Show Material materials with Elongación of 22.0 % | H111 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 25.0 % Show Material materials with Elongación of 25.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 26.0 % Show Material materials with Elongación of 26.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 26.0 % Show Material materials with Elongación of 26.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 29.0 % Show Material materials with Elongación of 29.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 29.0 % Show Material materials with Elongación of 29.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 32.0 % Show Material materials with Elongación of 32.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 32.0 % Show Material materials with Elongación of 32.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | H111 | EN 573-3 | Sheet, Strip | ||
20.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | H111 | EN 573-3 | Flat | A50 | |
Límite elástico | -270 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | H111 | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 |
-270.0 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | H111 | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 | |
20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | H111 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
20 MPa Show Material materials with Límite elástico of 20 MPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |||
20.0 °C | 20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | H111 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 20.0 - 60.0 MPa Show Material materials with Límite elástico of 20.0 - 60.0 MPa | H111 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | H111 | EN 573-3 | Rod, Tube, Flat | RP02 | |
20.0 °C | 20.0 - 55.0 MPa Show Material materials with Límite elástico of 20.0 - 55.0 MPa | H111 | EN 573-3 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube | RP02 | |
20.0 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | H111 | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 | |
20 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | H111 | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 | |
50.0 °C | 29.0 MPa Show Material materials with Límite elástico of 29.0 MPa | H111 | EN 573-3 | RP1 | ||
100 °C | 13.0 MPa Show Material materials with Límite elástico of 13.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP1 | |
100.0 °C | 27.0 MPa Show Material materials with Límite elástico of 27.0 MPa | H111 | EN 573-3 | RP1 | ||
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |||
20.0 °C | 25.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 26.5 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 25.0 - 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 25.9 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 25.9 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 25.9 - 26.5 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
Módulo elástico | -270 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
-195.0 °C | 78.4 GPa Show Material materials with Módulo elástico of 78.4 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
-85.0 °C | 73.5 GPa Show Material materials with Módulo elástico of 73.5 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
-30.0 °C | 71.4 GPa Show Material materials with Módulo elástico of 71.4 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Módulo elástico of 60.0 - 70.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
100.0 °C | 68.0 - 68.6 GPa Show Material materials with Módulo elástico of 68.0 - 68.6 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
100.0 °C | 68.6 GPa Show Material materials with Módulo elástico of 68.6 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
150.0 °C | 66.0 - 66.5 GPa Show Material materials with Módulo elástico of 66.0 - 66.5 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
150.0 °C | 66.5 GPa Show Material materials with Módulo elástico of 66.5 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
250.0 °C | 56.0 - 57.0 GPa Show Material materials with Módulo elástico of 56.0 - 57.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
250.0 °C | 56.0 GPa Show Material materials with Módulo elástico of 56.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
300 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Resistencia a la tracción | 60.0 MPa Show Material materials with Resistencia a la tracción of 60.0 MPa | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
65.0 MPa Show Material materials with Resistencia a la tracción of 65.0 MPa | H111 | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 60.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 60.0 - 95.0 MPa | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 65.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 95.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 65.0 MPa Show Material materials with Resistencia a la tracción of 65.0 MPa | H111 | EN 573-3 | Rod, Sheet, Strip, Tube | ||
20.0 °C | 65.0 - 95.0 MPa Show Material materials with Resistencia a la tracción of 65.0 - 95.0 MPa | H111 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Coil, Sheet, Strip | ||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | ||
0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Ángulo de flexión a 90° | 0 °/t Show Material materials with Ángulo de flexión a 90° of 0 °/t | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 899.0 - 900.0 J/(kg·K) Show Material materials with Calor específico of 899.0 - 900.0 J/(kg·K) | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 899.0 J/(kg·K) Show Material materials with Calor específico of 899.0 J/(kg·K) | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
Coeficiente de dilatación térmica | -50 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | 20-100°C | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4399999999999997e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5399999999999997e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | ||
20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 220.0 W/(m·K) | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 210.0 - 229.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 229.0 W/(m·K) | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 220.0 - 229.0 W/(m·K) Show Material materials with Conductividad térmica of 220.0 - 229.0 W/(m·K) | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
20.0 °C | 229.0 W/(m·K) Show Material materials with Conductividad térmica of 229.0 W/(m·K) | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | ||
Temperatura de fusión | 646.0 - 657.0 °C Show Material materials with Temperatura de fusión of 646.0 - 657.0 °C | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 34000000.0 - 36000000.0 S/m Show Material materials with Conductividad eléctrica of 34000000.0 - 36000000.0 S/m | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Conductividad eléctrica of 34800000.0 - 36000000.0 S/m | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | |
Resistividad eléctrica | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.78e-08 - 2.94e-08 Ω·m | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.9e-08 Ω·m | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | ||
20.0 °C | 2.8e-08 - 2.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.8e-08 - 2.9e-08 Ω·m | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube | |
20.0 °C | 2.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 Ω·m | H111 | EN 573-3 | Rod, Sheet, Flat, Strip, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.5 % Show Material materials with Aluminio of 99.5 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar |
Boro | 0.05 Show Material materials with Boro of 0.05 | H111 | EN 573-3 | Flat |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar |
0.05 % Show Material materials with Cobre of 0.05 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
Cromo | 0.01 Show Material materials with Cromo of 0.01 | H111 | EN 573-3 | Flat |
Galio | 0.03 Show Material materials with Galio of 0.03 | H111 | EN 573-3 | Flat |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H111 | EN 573-3 | Flat, Rod, Sheet, Strip, Tube |
0.40 % Show Material materials with Hierro of 0.40 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
0.4 % Show Material materials with Hierro of 0.4 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
Magnesio | 0.03 % Show Material materials with Magnesio of 0.03 % | H111 | EN 573-3 | Flat |
0.05 % Show Material materials with Magnesio of 0.05 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar | |
0.05 % Show Material materials with Magnesio of 0.05 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
Manganeso | 0.01 % Show Material materials with Manganeso of 0.01 % | H111 | EN 573-3 | Flat |
0.05 % Show Material materials with Manganeso of 0.05 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar | |
0.05 % Show Material materials with Manganeso of 0.05 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
Níquel | 0.03 Show Material materials with Níquel of 0.03 | H111 | EN 573-3 | Flat |
Otro | 0.03 % Show Material materials with Otro of 0.03 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | H111 | EN 573-3 | Flat |
0.25 % Show Material materials with Silicona of 0.25 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar | |
0.25 % Show Material materials with Silicona of 0.25 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | H111 | EN 573-3 | Flat |
0.05 % Show Material materials with Titanio of 0.05 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar | |
0.05 % Show Material materials with Titanio of 0.05 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip | |
Vanadio | 0.03 Show Material materials with Vanadio of 0.03 | H111 | EN 573-3 | Flat |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | H111 | EN 573-3 | Flat |
0.07 % Show Material materials with Zinc of 0.07 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Flat, Rod, Sheet, Strip, Tube, Plate, Foil, Bar | |
0.07 % Show Material materials with Zinc of 0.07 % | H111 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2, EN 546-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Lithography; Cable Wrapping: Electric cable wrapping; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, rotor hub, stairs; Cosmetics: Cosmetics pieces; Automotive Trim: Interior Trim, Marque Badges; Components: Heat shields, General Transportation | |
Brazing | Excellent | |
Corrosion properties | Excellent | |
Welding | Excellent | |
Workability | Excellent |