General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
2.705 g/cm³ Show Material materials with Densidad of 2.705 g/cm³ | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Medidas
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Dureza Brinell | 28.0 [-] Show Material materials with Dureza Brinell of 28.0 [-] | H12 | EN 573-3, EN 485 | Plate, Rod | |
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 |
4.0 % Show Material materials with Elongación of 4.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
7.0 % Show Material materials with Elongación of 7.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
9.0 % Show Material materials with Elongación of 9.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
9.0 % Show Material materials with Elongación of 9.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | ||
20.0 % Show Material materials with Elongación of 20.0 % | H12 | EN 573-3, EN 1715-2 | Plate, Rod | A50 | |
Módulo de cizallamiento | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Resistencia a la tracción | 85.0 - 125.0 MPa Show Material materials with Resistencia a la tracción of 85.0 - 125.0 MPa | H12 | EN 573-3, EN 485 | Plate, Rod | |
95.0 - 110.0 MPa Show Material materials with Resistencia a la tracción of 95.0 - 110.0 MPa | H12 | EN 573-3, EN 1715-2 | Plate, Rod | ||
Ángulo de flexión a 180° | 0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | |
1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | ||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | |
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | ||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | ||
3 °/t Show Material materials with Ángulo de flexión a 90° of 3 °/t | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | 20-100°C | |
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
225.0 - 235.0 W/(m·K) Show Material materials with Conductividad térmica of 225.0 - 235.0 W/(m·K) | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |||
234 W/(m·K) Show Material materials with Conductividad térmica of 234 W/(m·K) | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |||
Temperatura de fusión | 645.0 - 657.0 °C Show Material materials with Temperatura de fusión of 645.0 - 657.0 °C | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 35400000.0 - 36500000.0 S/m Show Material materials with Conductividad eléctrica of 35400000.0 - 36500000.0 S/m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
36000000.0 S/m Show Material materials with Conductividad eléctrica of 36000000.0 S/m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
Resistividad eléctrica | 2.74e-08 - 2.82e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.74e-08 - 2.82e-08 Ω·m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
2.78e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.78e-08 Ω·m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
4.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.9e-08 Ω·m | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.5 % Show Material materials with Aluminio of 99.5 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Boro | 0.05 % Show Material materials with Boro of 0.05 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.05 % Show Material materials with Cobre of 0.05 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Cromo | 0.01 % Show Material materials with Cromo of 0.01 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.01 % Show Material materials with Cromo of 0.01 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Galio | 0.03 % Show Material materials with Galio of 0.03 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.4 % Show Material materials with Hierro of 0.4 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Manganeso | 0.01 % Show Material materials with Manganeso of 0.01 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.01 % Show Material materials with Manganeso of 0.01 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Otro | 0.1 % Show Material materials with Otro of 0.1 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.1 % Show Material materials with Silicona of 0.1 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.05 % Show Material materials with Zinc of 0.05 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | Good (For surface protection only) | |
Application areas | Conductors; rods for the manufacture of aluminium conductor wires. | |
Brazing | Excellent | |
Corrosion properties | Very Good | |
Welding | Very Good | |
Workability | Very Good |