General
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
2.705 g/cm³ Show Material materials with Densidad of 2.705 g/cm³ | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Dureza Brinell | 34.0 [-] Show Material materials with Dureza Brinell of 34.0 [-] | H14 | EN 573-3, EN 485 | Plate, Rod | |
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | H14 | EN 573-3, EN 485 | Plate, Rod | A50 |
4.0 % Show Material materials with Elongación of 4.0 % | H14 | EN 573-3, EN 485 | Plate, Rod | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | H14 | EN 573-3, EN 485 | Plate, Rod | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 485 | Plate, Rod | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | H14 | EN 573-3, EN 485 | Plate, Rod | ||
14.0 % Show Material materials with Elongación of 14.0 % | H14 | EN 573-3, EN 1715-2 | Plate, Rod | A50 | |
Módulo de cizallamiento | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | |||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Resistencia a la tracción | 105.0 - 145.0 MPa Show Material materials with Resistencia a la tracción of 105.0 - 145.0 MPa | H14 | EN 573-3, EN 485 | Plate, Rod | |
115.0 - 130.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 130.0 MPa | H14 | EN 573-3, EN 1715-2 | Plate, Rod | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | Plate, Rod | |
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Plate, Rod | |
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Plate, Rod | ||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | Plate, Rod | ||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Plate, Rod |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
Conductividad térmica | 225.0 - 235.0 W/(m·K) Show Material materials with Conductividad térmica of 225.0 - 235.0 W/(m·K) | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
234 W/(m·K) Show Material materials with Conductividad térmica of 234 W/(m·K) | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |||
Temperatura de fusión | 645.0 - 657.0 °C Show Material materials with Temperatura de fusión of 645.0 - 657.0 °C | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 35400000.0 - 36500000.0 S/m Show Material materials with Conductividad eléctrica of 35400000.0 - 36500000.0 S/m | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
36000000.0 S/m Show Material materials with Conductividad eléctrica of 36000000.0 S/m | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
Resistividad eléctrica | 2.74e-08 - 2.82e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.74e-08 - 2.82e-08 Ω·m | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
2.78e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.78e-08 Ω·m | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 99.5 % Show Material materials with Aluminio of 99.5 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Boro | 0.05 % Show Material materials with Boro of 0.05 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Cromo | 0.01 % Show Material materials with Cromo of 0.01 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Galio | 0.03 % Show Material materials with Galio of 0.03 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Hierro | 0.40 % Show Material materials with Hierro of 0.40 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Manganeso | 0.01 % Show Material materials with Manganeso of 0.01 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Zinc | 0.05 % Show Material materials with Zinc of 0.05 % | H14 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |