General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.81 g/cm³ Show Material materials with Densidad of 2.81 g/cm³ | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 160.0 MPa Show Material materials with Bending Fatigue Strength of 160.0 MPa | T6 | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||
Dureza Brinell | 150.0 [-] Show Material materials with Dureza Brinell of 150.0 [-] | T6 | AA Standards | |
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||
Resistencia a la tracción | 450.0 MPa Show Material materials with Resistencia a la tracción of 450.0 MPa | T6 | AA Standards, ASTM B247 | |
455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T6 | AA Standards, ASTM B247 | ||
470.0 MPa Show Material materials with Resistencia a la tracción of 470.0 MPa | T6 | AA Standards, ASTM B247 | ||
475.0 MPa Show Material materials with Resistencia a la tracción of 475.0 MPa | T6 | AA Standards, ASTM B247 | ||
485.0 MPa Show Material materials with Resistencia a la tracción of 485.0 MPa | T6 | AA Standards, ASTM B247 | ||
490.0 MPa Show Material materials with Resistencia a la tracción of 490.0 MPa | T6 | AA Standards, ASTM B247 | ||
495.0 MPa Show Material materials with Resistencia a la tracción of 495.0 MPa | T6 | AA Standards, ASTM B247 | ||
505.0 MPa Show Material materials with Resistencia a la tracción of 505.0 MPa | T6 | AA Standards, ASTM B247 | ||
510.0 MPa Show Material materials with Resistencia a la tracción of 510.0 MPa | T6 | AA Standards, ASTM B209, ASTM B247 | ||
515.0 MPa Show Material materials with Resistencia a la tracción of 515.0 MPa | T6 | AA Standards, ASTM B247 | ||
525.0 MPa Show Material materials with Resistencia a la tracción of 525.0 MPa | T6 | AA Standards, ASTM B209 | ||
530.0 MPa Show Material materials with Resistencia a la tracción of 530.0 MPa | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B316 | ||
540.0 MPa Show Material materials with Resistencia a la tracción of 540.0 MPa | T6 | AA Standards, ASTM B209, ASTM B221, ASTM B241 | ||
560.0 MPa Show Material materials with Resistencia a la tracción of 560.0 MPa | T6 | AA Standards, ASTM B221, ASTM B241 | ||
570.0 MPa Show Material materials with Resistencia a la tracción of 570.0 MPa | T6 | AA Standards |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium | |||
Coeficiente de dilatación térmica | 20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 | ||
Conductividad térmica | 130 W/(m·K) Show Material materials with Conductividad térmica of 130 W/(m·K) | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 | ||
Temperatura de fusión | 475.0 - 635.0 °C Show Material materials with Temperatura de fusión of 475.0 - 635.0 °C | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Eléctrico
Property | Value | Condition | Related Standards |
---|---|---|---|
Conductividad eléctrica | 19000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 S/m | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Resistividad eléctrica | 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 Ω·m | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 1.2 - 2.0 % Show Material materials with Cobre of 1.2 - 2.0 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Cromo | 0.18 - 0.28 % Show Material materials with Cromo of 0.18 - 0.28 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Magnesio | 2.1 - 2.9 % Show Material materials with Magnesio of 2.1 - 2.9 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Manganeso | 0.3 % Show Material materials with Manganeso of 0.3 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Zinc | 5.1 - 6.1 % Show Material materials with Zinc of 5.1 - 6.1 % | T6 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B316 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), good to acceptable | |
Workability | general (condition): not suitable |