General
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T732 | EN 573-3 | Profile | ||
Módulo de cizallamiento | 27.1 GPa Show Material materials with Módulo de cizallamiento of 27.1 GPa | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 25.0 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 25.0 - 27.0 GPa | T732 | EN 573-3 | Profile | ||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 70.0 - 73.0 GPa Show Material materials with Módulo elástico of 70.0 - 73.0 GPa | T732 | EN 573-3 | Profile | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Resistencia a la tracción | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T732 | EN 573-3 | Profile |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 862.0 J/(kg·K) Show Material materials with Calor específico of 862.0 J/(kg·K) | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 862.0 J/(kg·K) Show Material materials with Calor específico of 862.0 J/(kg·K) | T732 | EN 573-3 | Profile | |
Coeficiente de dilatación térmica | -50 °C | 2.16e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.16e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile |
-50.0 °C | 2.16e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.16e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
20 °C | 2.16e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.16e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.43e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
20 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3399999999999996e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100.0 °C | 2.34e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.34e-05 1/K | T732 | EN 573-3 | Profile | |
200 °C | 2.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.43e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
200.0 °C | 2.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.43e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
300 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
300.0 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Profile | |
Conductividad térmica | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 160.0 W/(m·K) | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Temperatura de fusión | 480.0 - 640.0 °C Show Material materials with Temperatura de fusión of 480.0 - 640.0 °C | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 19000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 23000000.0 S/m | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Resistividad eléctrica | 4.35e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 - 5.26e-08 Ω·m | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 1.2 - 2.0 % Show Material materials with Cobre of 1.2 - 2.0 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Cromo | 0.18 - 0.28 % Show Material materials with Cromo of 0.18 - 0.28 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T732 | EN 573-3 | Profile |
0.50 % Show Material materials with Hierro of 0.50 % | T732 | EN 573-3, EN 603 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Magnesio | 2.1 - 2.9 % Show Material materials with Magnesio of 2.1 - 2.9 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Manganeso | 0.3 % Show Material materials with Manganeso of 0.3 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Zinc | 5.1 - 6.1 % Show Material materials with Zinc of 5.1 - 6.1 % | T732 | EN 573-3, EN 603 | Profile, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: not suitable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient to poor, weathering: sufficient to poor | |
Workability | Bending / Spinning (cold): sufficient (O) / not suitable, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) not suitable / not suitable |